Re: [MW:34881] Re: 14478] QW-403.6 OF ASME SEC. IX (MIN. THK. RANGE QUALIFICATION)

Your SMAW thick 20mm , lower limit is 16mm and higher limit 40mm. So your existing PQR not qualified.

D.V.reddy.

On Mon, 15 Apr 2024, 8:23 pm arung...@gmail.com, <arung22.4u@gmail.com> wrote:
Dear all,

I have a question:

We currently have a Welding Procedure Specification (WPS) and Procedure Qualification Record (PQR) for welding a 25mm plate using a combination of Gas Tungsten Arc Welding (GTAW) and Shielded Metal Arc Welding (SMAW), with impact testing conducted. The weld metal deposited by GTAW is 5mm, and SMAW is 20mm.

Now, if I only intend to use the SMAW process for welding 8mm and 15mm thick plates, both requiring impact testing, would our existing WPS still qualify for this welding scenario?


On Thursday, June 7, 2012 at 5:19:11 PM UTC+3 John Henning wrote:

Minimum thickness is 6mm.

 

QW-403.6 says ". . . where T is less than 6mm, the minimum thickness qualified is 1/2T . . ." .   Since your thickness is not less than the general rule of T to 2T applies.

 

Note this wording has also given me heart burn.  What I have done is to take a 1/4 inch plate (nominally 6mm) and have the thickness machined to 0.249 inches, this then qualifies for thickness 0.124 to 0.499 inches.  If I need the thickness I will also weld a 1/2 inch thick plate to qualify 1/2 to 1 inch. 

 

Enjoy.

 

John A. Henning

Welding & Materials

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of CHINTUKUMAR GANDHI
Sent: Wednesday, June 06, 2012 5:30 AM
To: material...@googlegroups.com
Subject: [MW:14478] QW-403.6 OF ASME SEC. IX (MIN. THK. RANGE QUALIFICATION)

 

Dear Experts,

 

What shall be the minm. qualified thk. range if PQR is qualified with 6 mm. Nom. thk. with Notch toughness properties. Will it be 3 mm. or 6 mm. as per QW-403.6 of ASME Sec. IX?

 

Further, suppose If I shall qualify this procedure on 5 mm. thk. PQR test coupon (machined from 6 mm. thk.), which thickness shall I have to consider for temperature reduction during subsize test specimen testing? Will it be 5 mm.(actual thk.) or 6 mm. (nom. thk.)?

 

Awaiting your experts' opinion at the earliest.

 

Thanks & regards,

 

 

C. R. GANDHI

 

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1263858d-e33f-4a21-8823-c75afd47ddean%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEabyK%3D5cT_J0S481hoL-EcDM8sugaOtRAGwDFU%2BsypumR3_gQ%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...