For GTAW welding  -Single Vee - 33.4 OD, Full GTAW welding  - 
SS TO SS Welding   or Cr > 3 %  , backing gas is required to get sound root without any Oxidation.
The Oxygen is excluded by  purging Argon/Helium or other Inert mixtures  at root side to avoid Oxidation .
The root side is inaccessible  due to small diameter in your above case.
Backing gas shall be continued till 6mm deposit is welded . This is not a Code requirement but followed  as a good engineering practice across industries 

Thanks 
Vishwas 

On Monday, May 22, 2023 at 4:51:37 PM UTC+5:30 Anand Elankumaran wrote:
Hi Mr. Vishwas Keskar,

Single Vee butt weld  - Root/Hot/fill/cap-  full GTAW

pipe OD -33.4 mm

On Mon, May 22, 2023 at 7:47 AM Vishwas Keskar <vvkes...@gmail.com> wrote:
Are you intending to qualify PQR in 
Single Vee butt weld - No welding from Root side ?
Double Side Weld with back grinding DPT from root side ?
This will decide the PQR  purging requirement

Thanks

Vishwas
IWE 


Sent from my iPhone

On 22-May-2023, at 8:40 AM, Anand Elankumaran <email2...@gmail.com> wrote:


Dear experts,

Could you please check and advise the below query.

  • Whether the back purging is a quality requirement or the ASME code is insisting on back purging on SS material while doing the GTAW process.
  • Whether we can qualify SS -GTAW PQR without back purging or the ASME code does not allow doing PQR for austenitic steels without a back purge?
  • Kindly advise how to do it without purging in SS GTAW Welding . Planning for PQR as well 


--
Thanks and Regards,
E. Anand,
Lead QA-QC,
Sohar,
Oman.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANOYChxEbF6gP%2BwCFusuTWnJpmbZMst%2BM1qCz3y2fHr0mRaY1Q%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.


--
Thanks and Regards,
E. Anand,
Lead QA-QC,
Sohar,
Oman.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/81326b99-027e-4e94-855a-f41ac118514cn%40googlegroups.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...