Hi
I did not get any chance to do research on the effect of ferrite content on SS to answer your question exactly, however I found one welding journal related to this discussion, attached herewith for reference.
Specific case study : The elevated-temperature mechanical properties of weld metal with a wide delta ferrite range are determined following their deposition using E308-16 covered electrodes.
There may be many studies available like this
There is brief explanation given in TWI page as below link,
https://www.twi-global.com/technical-knowledge/job-knowledge/welding-of-austenitic-stainless-steel-103/if ferrite is more than 10, what will happenTHANKS & BEST REGARDS,KG.PANDITHAN, BE, IWE, AWS-CWI, CSWIP 3.1,CONSULTANT-WELDING & QUALITYMobile no: +919940739349On Wed, Apr 11, 2018 at 4:24 PM, George Dilintas <dilintas@gmail.com> wrote:all this when MDMT is colder that -196degC and if the base metal is 316L and if the process is GTAW or GMAW--2018-04-11 8:34 GMT+03:00 Ramesh <rameshkannandevaraj@gmail.com> :
On Wed, Apr 11, 2018 at 9:12 AM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:Could you elaborate the mechanism of Hot cracks if ferrite is less than 3THANKS & BEST REGARDS,KG.PANDITHAN, BE, IWE, AWS-CWI, CSWIP 3.1,CONSULTANT-WELDING & QUALITYMobile no: +919940739349On Tue, Apr 10, 2018 at 10:10 PM, PREM SHANKARDUTT NAUTIYAL <prem_nautiyal@rediffmail.com> wrote:Ferrite number less than 3 can result in hot cracks in ASS.
Regards
Prem Nautiyal
PREM S NAUTIYAL
CELL : 9769316004
From: Kannayeram Gnanapandithan <kgpandithan@gmail.com>
Sent: Tue, 10 Apr 2018 18:11:30 GMT+0530
To: materials-welding <materials-welding@googlegroups.com >
Subject: Re: [BULK] [MW:27668] Stainless steel (SA 312 TP 316L) weldingwhat is the reason for Hot crackingTHANKS & BEST REGARDS,KG.PANDITHAN, BE, IWE, AWS-CWI, CSWIP 3.1,CONSULTANT-WELDING & QUALITYMobile no: +919940739349On Tue, Apr 10, 2018 at 4:51 PM, Lu, Feng <luf@zachrygroup.com> wrote:3 ~ 8% ferrite are required in the weld to prevent hot cracking
Feng Lu, Ph.D., NDE Level III
Metallurgy and Welding Engineer
Zachry Industrial, Inc.
3600 West Sam Houston Pkwy Southluf@zachrygroup.com
Office: 713.979.2648
Cell: 512 797 5777
www.ZachryGroup.comThis e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message.
From: materials-welding@googlegroups
.com [mailto:materials-welding@googlegroups.com ] On Behalf Of Kannayeram Gnanapandithan
Sent: Tuesday, April 10, 2018 5:56 AM
To: materials-welding <materials-welding@googlegroups.com >
Subject: [BULK]Re: [MW:27666] Stainless steel (SA 312 TP 316L) welding
what is the necessity for ferrite testing on 316L
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE, AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349
On Tue, Apr 10, 2018 at 4:16 PM, Perumal Govindan <perumalgovindan@gmail.com> wrote:
Hi Prasad,
Ferrite testing is required when it is mentioned in the Client / Project Welding / Construction Specification.
With Kind Regards
P Govindan
On Tue, Apr 10, 2018 at 11:24 AM, 'Shashank Vagal' via Materials & Welding <materials-welding@googlegroup
s.com > wrote:NO
On Sunday, 8 April 2018 6:41 PM, Prasad Rode <purode333@gmail.com> wrote:
Dear sir,
I am going to do PQR for SA 312 TP 316L pipe to pipe of 6" and 7.11mm thickness.
I want to know that, i have to go for ferrite testing or not ?
If not, when it is essential to ferrite testing?
Regards
Prasad
--
https://materials-welding.blogspot.com/ 
https://secure-web.cisco.com/1YQnsmRr-GH1GARoxWXMeA5C-zFwTzL octJUEMDdbzGqdXz0x9TjaAPfvUNCL PyWmBF72X02uczwD2w2oQr4w1WU83Q i9TlzHiZ7Q_m9togWnC_PifpMYG8No h8ecDgt7Rz98rlzdDCP25FnmnS_fTs bYKEW23twpN4Bzour50n0apwtEnAxZ YN9sAWmkWYerjHTOdoPgbEeCq6R1Ta DdAKBlmlFHT4VODFg8bxr_Ky0_qRNk uh067eU3nfDwrJG-XJiwtMxynCYDVI ZxQz1Fv74pM0X3HjGhj247CNngXDfo Nc61SRf3RPhE2b34P5EiGja9P9JH-O sWp5vdlOZ_ev82Kyia9HdDn4kwpU9b D_Y/https%3A//www.linkedin.com %2Fgroups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://secure-web.cisco.com/1-hvkRaP05ZCIdzs4SHsFJNT9bNun5i .t9Jd9i_VDkw1AUQnt1B_8PvkK-5KPs sj1ExOaVPMda4kh79O3-nwhzRckMK5 PNlvmAX3tP3s8UcQbpjY4u6F98DxOZ _fH7AtzprQyB5Qhj6i06A2Vtf5DvTM zg0taC8VPuylTiEN6kray-J6mSH7rD 5orTEuXBUqWHY0XJTUW8BT0jVxHDa8 Mpq1J4R8qbvoEgMl3fZ2yaI2GQWyc5 7xv9U6uF_6RuNqso_Kl_aOOPXwGTep m00WRQkCkB5IN5Bbp3nDX7n3z5YuRF aa6YDUiw3XQ4qTR9dNndOcf4Tb3V5C qSc8r4GTxyOJ_rqisrNgGsTqnWuuQ8 S-A/https%3A%2F%2Fgroups.googl e.com%2Fgroup/materials-weldin g 
For more options, visit https://secure-web.cisco.com/11LbN4v-1Vdxbtx9wzmvNLlrp8uw6D6 .6SWirlI5SOn-YhcHDPOM5GhE6va5qK kPm_WjdJVCXM_Ev0AsJwnBggZ71lDF T-ump4X6eoB8B9kDI9imYMY1Egx6DH IGG4asTwbZiikNoMyLvIZn2hRyxaMg kPyo-CYZYNykefeET8HwTcUVqQBEPj S-MTu7OmiuqtRe_zpIH1qMlNrjblAu JjS5Uz1SGGxHGmAE3j0SIPzjn5ZXKA TiqNlyDVZxWCkTaz4Cv6gLjf9aK7Sd 1OpQJkIAcpioyy8RD5qUkbwU9Ixs21 FggLi3SNukHhJ3H-XBnX9R3JDCs3Nf gZ3Olgx0BzW2UewBza6kNw3toz3lk6 w6E/https%3A%2F%2Fgroups. google.com%2Fd%2Foptout 
--
https://materials-welding.blogspot.com/ 
https://secure-web.cisco.com/1YQnsmRr-GH1GARoxWXMeA5C-zFwTzL octJUEMDdbzGqdXz0x9TjaAPfvUNCL PyWmBF72X02uczwD2w2oQr4w1WU83Q i9TlzHiZ7Q_m9togWnC_PifpMYG8No h8ecDgt7Rz98rlzdDCP25FnmnS_fTs bYKEW23twpN4Bzour50n0apwtEnAxZ YN9sAWmkWYerjHTOdoPgbEeCq6R1Ta DdAKBlmlFHT4VODFg8bxr_Ky0_qRNk uh067eU3nfDwrJG-XJiwtMxynCYDVI ZxQz1Fv74pM0X3HjGhj247CNngXDfo Nc61SRf3RPhE2b34P5EiGja9P9JH-O sWp5vdlOZ_ev82Kyia9HdDn4kwpU9b D_Y/https%3A//www.linkedin.com %2Fgroups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://secure-web.cisco.com/1-hvkRaP05ZCIdzs4SHsFJNT9bNun5i .t9Jd9i_VDkw1AUQnt1B_8PvkK-5KPs sj1ExOaVPMda4kh79O3-nwhzRckMK5 PNlvmAX3tP3s8UcQbpjY4u6F98DxOZ _fH7AtzprQyB5Qhj6i06A2Vtf5DvTM zg0taC8VPuylTiEN6kray-J6mSH7rD 5orTEuXBUqWHY0XJTUW8BT0jVxHDa8 Mpq1J4R8qbvoEgMl3fZ2yaI2GQWyc5 7xv9U6uF_6RuNqso_Kl_aOOPXwGTep m00WRQkCkB5IN5Bbp3nDX7n3z5YuRF aa6YDUiw3XQ4qTR9dNndOcf4Tb3V5C qSc8r4GTxyOJ_rqisrNgGsTqnWuuQ8 S-A/https%3A%2F%2Fgroups.googl e.com%2Fgroup/materials-weldin g 
For more options, visit https://secure-web.cisco.com/11LbN4v-1Vdxbtx9wzmvNLlrp8uw6D6 .6SWirlI5SOn-YhcHDPOM5GhE6va5qK kPm_WjdJVCXM_Ev0AsJwnBggZ71lDF T-ump4X6eoB8B9kDI9imYMY1Egx6DH IGG4asTwbZiikNoMyLvIZn2hRyxaMg kPyo-CYZYNykefeET8HwTcUVqQBEPj S-MTu7OmiuqtRe_zpIH1qMlNrjblAu JjS5Uz1SGGxHGmAE3j0SIPzjn5ZXKA TiqNlyDVZxWCkTaz4Cv6gLjf9aK7Sd 1OpQJkIAcpioyy8RD5qUkbwU9Ixs21 FggLi3SNukHhJ3H-XBnX9R3JDCs3Nf gZ3Olgx0BzW2UewBza6kNw3toz3lk6 w6E/https%3A%2F%2Fgroups. google.com%2Fd%2Foptout 
--
https://materials-welding.blogspot.com/ 
https://secure-web.cisco.com/15CdaQ7SqBttaMDjEgp4vyA1IIjLruZ 4x02m8Ah9pYq6pSUFOK4-lHzhH7m7k 9MIiS0unxn4qfOA70v59vOPWRGhNUr ugmrLXvQ-X0WNEztRVJR8_iUnWuJL7 ZngVRii6W0MHgWbayD58uOybu_o_WS 7TXJfyWs-_7Fy3RGrk262seUpeYMyB OkVy6JjNeidtV2NikbqfRJ69VudWHl R7Pj1brCz_pmBZyqwiAvBxYfKg2Uu8 IxnyW6iurEV6LnqgTLG1l95kaOCk5T 8n2-t1_mZz0HXQowSp2KjuOD4Zb7Zn lfDrumTmHmUIr_DltelYqkudojkTlc FiSo_OS8RBn7ObjA0peImqj_vGZwZA 27Y/https://www.linkedin.com/g roups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://secure-web.cisco.com/1eRh-wf9X8OZeiSzdXfjjdBsreEz2vw .6nypbfDtNb9gF9ga2ioNVBw6jsStnX 7fBTJt1ESgLZHyRIrp3TXqnx28FIbM h1w8a3F8es4N0JYiKyPOeTKWWkEa9I IqUXxQ9P-Fjen_zx8xXb2UfxCrDNSa tnz7YR3tcclkVDWvUGZWNSCxsHhWey 9xdfpJ4q6yxf0Nphl2FTNTbt1uzeSb cMh-d1-maJnFMgDZv-W_0HKTlLLzJO pdn7ZZ0ojXZxwg2PSa2zxDZPuPyT49 Qzb49J-Vn5b1A5yVIfU6jLSqX01kz5 _VERtpsouoOvlyw_ExjdM_Rz3iU2Cv SdWr3y5LILETR4FgI0PysBwPO2uVgB q70/https%3A%2F%2Fgroups.googl e.com%2Fgroup/materials-weldin g 
For more options, visit https://secure-web.cisco.com/1Gqw5l2Ew0NnLF9ocT7FiPSzoc7Xh5I .XXL0ZUUCS2kBzZm-hHDlnrap_v-m_b jpNstyVad2i7EysoEtlOT4Te7ttRG- bQ3cta-FkTGYTXN1OiukqlCyELfHfF -mW95cAi6BWn-5VkwmqdM0MqNz5Gay Yxa_NlqaaeBiPR599qfT5pB4k82oN1 UntSTlKDSO21R7GS84NHR7QhdtV8Jk 8SnQeqMqgFiGqQ0xp6ZLe2oxwCz-6n -dTkyCYepQifCb4HSm2SkrJ5jla3kc WsKsa-GWg2J_u_WEMlfVJBriXkMRO9 IQQ_2t-pZATcoezLzmb-EKYYb9PEqD sTxFrV5cu-lMxRMUoWqyFeOy10TFMt T90/https%3A%2F%2Fgroups.googl e.com%2Fd%2Foptout 
--
https://secure-web.cisco.com/1Yekz4_Rk1j5eIKzWu3w3uOI4lY_995 nOXaYoO2uO0NGqMQXH-ZV9VapwaVCb 3IxXLLVZM8kjdu9fM7j1srk-jOXoit pI_KNfy6y596DmYrln7EAsMlF7l9hP mw01eSNbToT4y3p6Ek5qnqPiaII6IA qGJkGpUWHzaHjuP-_HJSX4av0Zg1Tx LLPqX1jOpfkdDwcIKu_Ch0W90jC3sj e2nKE3fvQdvq-EYXWuoP2PhBkY0GXw Y1i2E3lGsFgt1uDo9QhRi4zd7373nA XJj-tQQipR7ApVH3skfaHyElP254Ze HlSze7RhOtIpzCm5v8VlQA1BgwYbg4 CwFlK0wOolWVMJxCeqE-36laFK69SE hm4/https://materials-welding. blogspot.com/ 
https://secure-web.cisco.com/1T4WuM8lkw7TepJTiGMw6aWBwIYmQBs eyjuGtIJoulgjhLZ7EVw-eED0B1_yt TaqgwjwuKfJDC_-XzBITrF66Tr4OYo TqxRHrf5DQUoEx9xJI6uGsnT6T8rqf 0HxLaPaKsrwqTgORJ2twvVMj_3SiNn hcIVIjbcKSjdNG1FQeNdUJGX4QZfXd CfYnvWOC5GWgApzenhyd2_29Hux1Dp znKaRGakrq7I4wwOMAWVHQWE8OCzrY h7nIOtoZyGlAtn7VO4zhFjdXFddWZv 8zbXOxkuYVLcN_iktDQ4QjpF2OH1ol C3Yq6cQppUBAbQyMxLeGmFekICOzEP KI77xUxO43Tj1RtqibnEb207n4J3s- 0nU/https:%2F/www.linkedin.com %2Fgroups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://secure-web.cisco.com/1Ngm51h-0qXokcX3NLuwji6oaxruW94 .TI5tEOmO1aty65EiLOKKAcQAr68Fvw Vf78F6_OtvN32tWU5Lo4oA7s1YkEXv 0OHLp81p0sCofVtvL_oIeFWNNKGcv9 iMdNcwMXXDzGifLIWiQ48hFHkxVInM wZlGnja2s_d_WvL4H0v6n1hcxmdWA3 GGn6jMV6d-GX_POXR9hO9uph_XZEpT i7PoWXy1sD6lkIPzr-5dP_L915H9wV 0bQQbrS25sQGTV_SiLNRP6rUQrKepR KanOk-bjnvEJU4he9cvr5z5caUHBx0 dzFDnJCTVD8sFrYcqLvuy20Uqus58- v-T5mqQfVcEFY9DZFq4rxHOd50h0hv QLM/https%3A%2F%2Fgroups.googl e.com%2Fgroup%2Fmaterials-weld ing 
For more options, visit https://secure-web.cisco.com/1-QRVl4sxcfjWZp6YgOWKAKJzKAlR_7 .F_l7FBH2DlcrNxj28971TvyG3D9TUY 7yjqDSQpFDD1cnUDClMxcS5LTpP2yZ TAwaIS0TZaWVPLssYGuKtKb1E0XqEN Y9Rsfh6_ETm2-nUYG3JD_dMZ2IsaFk hc8gkZ8mttKHmSf7i-6Kp6uRv3mlB4 3KECYM1LxTVCM82pSlZsp8WEmqWAqK DOL2xJ84gtaQQCIZM7zYrZZN1QEiGH Uw5VvY3eT0B7MpjQ_mhtwqJkV4AUGA pHdPioxXJ8XxQweNrThd9aGwtrOYaf 1lV6zwy9Ub2_nSCbcsN81Tem-OjoMa bJVULfpk9qctXstwFam_Z-NakErpuQ k7w/https%3A%2F%2Fgroups.googl e.com%2Fd%2Foptout --
https://materials-welding.blogspot.com/ 
https://www.linkedin.com/groups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https:roups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
--
https://materials-welding.blogspot.com/ 
https://www.linkedin.com/groups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
--
https://materials-welding.blogspot.com/ 
https://www.linkedin.com/groups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
--
https://materials-welding.blogspot.com/ 
https://www.linkedin.com/groups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
--
https://materials-welding.blogspot.com/ 
https://www.linkedin.com/groups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
--Dr. Georgios Dilintas,Dipl. Ing. In Aeronautic and Space EngineeringPh.D in Mechanics of Solids - Computational MechanicsA.I.S, A.N.I, IRCA Lead AuditorWelding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis
https://materials-welding.blogspot.com/ 
https://www.linkedin.com/groups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
--
https://materials-welding.blogspot.com/ 
https://www.linkedin.com/groups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.



Comments