Skip to main content

[MW:25828] Re: For Cryogenic Services at Temp -196 degree Celsius (17 Kelvin) Pipe of ASTM 312 TP 304 L is suitable?

Dear experts,

For Cryogenic applications which involves Minor Welding, I would suggest to use SS304LN, SS316LN. I would say there no economical replacement for these grades with same properties.

They have excellent impact toughness values even at -196 degrees they would show more than 80J value.

But due care has to be taken during welding since these grades are susceptible for liquation cracking.

Thanks

Abhinandan Admuthe

Chief Metallurgist

Delta Metallurgical Laboratory
(AN ISO/IEC 17025:2005 Accredited Laboratory)
On Tuesday, December 6, 2016 at 8:37:06 AM UTC+5:30, viveksinghme1612 wrote:

Dear Experts,

Currently I am working on a project of ISRO (Indian Space Research Organisation) for Integrated Cryogenic Engine Testing Facility (ICET), for bidding in that services are Liquid Hydrogen, Liquid Oxygen, Liquid Helium, Liquid Nitrogen, Gaseous Hydrogen, Gaseous Oxygen, Gaseous Nitrogen, Gaseous Helium.

For SS Seamless Pipes client has given three options for material ASTM 312 TP 304L/ ASTM 312TP 316L/ ASTM 312TP 321. 

Kindly suggest me the suitable material for the same that gives economical and best design.


Thanks in advance.


Regards:-

Vivek Singh Chaudhary

Piping Design Engineer.

Contact No.- +91 9990441755.

Email :- viveksin...@gmail.com



--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/7d5b4787-f4ce-4b84-bd2d-a70c6a779c7e%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .