Hi,

You have to give full details like what was the no of layers, total height of cladding and what welding process was used for PQR etc.
When doing cladding, first layer will always be diluted. In your below email you have specified that you achieved undiluted chemistry at 3mm from weld interface. And client requirement is 2mm undiluted chemistry from top. In order to achieve this your welding should be 3mm (where you have achieved undiluted chemistry + 2mm minimum (client requirement) deposition.

Sent from my iPad

On 24-Dec-2015, at 15:03, 'Prakash Hegde' via Materials & Welding <materials-welding@googlegroups.com> wrote:

Hi!
It is very difficult to achieve at 1mm from fusion line the undiluted chemistry unless you go on grinding of layers at least twice which is not a good proposal in such case you qualify the PQR with utmost precaution of overlap and heat input and  get the approval from client .
Regards
Hegde


On Wednesday, 23 December 2015 4:14 PM, Vanchinath S.A. <vanchinaths@gmail.com> wrote:


If you are analysing by spectro it should meet at 1mm. Otherwise you take chips from 1mm to 3mm and analyse the chemistry and prove it meets the requirement. In my opinion 5mm WD is required to meet 2mm undiluted weld.  Vanchinath
On 23 Dec 2015 15:52, "'CHINTUKUMAR GANDHI' via Materials & Welding" <materials-welding@googlegroups.com> wrote:
Dear Experts, 

Greetings of the day. 

 I need your expert advise on an issue. In one of our project, 70-30 Cu-Ni W.D. to be done on P-No. 1 base metal. As per client's Data sheet, 3.0 mm. W.D. is specified. Accordingly we have qualified WPS to get the undiluted chemistry on 3 mm. W.D. from interface as per ASME Sec. IX. But in client's project spec. it is specified- "in case a higher deposition thickness and multiple weld layers are required to achieve the minimum specified undiluted deposit metal, the same shall be done only after taking prior approval of client. Minimum thickness of undiluted finished weld overlay from top shall be 2 mm. or as specified in the drawing. Now, my concern is shall we have to certify undiluted chemistry at 1 mm. from fusion surface considering (3 mm. required W.D. as per Data sheet - 2 mm.) or at 3 mm. viz. top surface. 

Please revert at the earliest. 

 Thanks & regards, 



 C. R. GANDHI
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1264702308.2732768.1450865939902.JavaMail.yahoo%40mail.yahoo.com?utm_medium=email&utm_source=footer.
For more options, visit https://groups.google.com/d/optout.
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CA%2B6Tn1%2BnY-QFMfxo7mMUBk0XFRATuz-LHFfff9o56Rvw%2BM9LRA%40mail.gmail.com?utm_medium=email&utm_source=footer.
For more options, visit https://groups.google.com/d/optout.


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/416352862.3027078.1450955027956.JavaMail.yahoo%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .