Dear Chandra,

 

You didn't give any details about the WPS and PQR availability for the HDPE Butt Fusion welding and following checks shall be done to ensure the quality,

 

1) 180 Deg Bend Test (4 pieces) for the 1st fusion joint per shift/day or any change in welding parameters like fusion temperature, time & pressure.

 

2) Check the Mismatch prior to start heating and fusion.

 

3) External Weld bead should be uniform for the both side.

 

4) Weld bead to be shaved to check the miss alignment or lack of fusion.

 
 
Regards,
 
Mohan, Q8.
 
 
 
 
 
 
 
 

 
On Tue, Feb 4, 2014 at 9:52 PM, Chandrasekar Rengasamy <chandrasekaraug@gmail.com> wrote:
Any Tips for HDPE Butt Fusion Welding
In Process Monitoring / weld Visual Inspection ....
to ensure good quality !!!

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
With Regards,

Mohan, Q8.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:35354] Cast-iron welding

1. Preheat joint area(other area, cover with mineral wool). 2. ENiCi or ENiFe-CI. 3. stringer bead. 4. peening is to be done on weldmetal im...