Re: [MW:20108] RE: Black spots on DSS Weld Joints.

Dear Sir,

We use Pure Argan  - 99.998%  with moisture <5PPM, Oxygen <5 PPM as per Gas MTC.

We use separate shop for DSS welding for avoiding contamination from CS welds/ grinding.

Welders aware of Acetone cleaning of joint, filler wires etc.

Purging gas  O2 level continuously monitored with instruments till completion of welding  (maintained <0.03%).

Random checks during welding  observed inter pass temp. some time more than 150 Deg.C  but <200 Deg.C

Some time we preheat to 50 Deg.C  to remove moisture.

This problem typically we observe in 6" & 8" Pipes, others are satisfactory (lower dia).


Is it dark spots are any inter metallics? ( As per leterature it forms at 300-700 Deg.C, generally during welding, this range not encountered).

Pickling & Passivation will be costlier, management may reluctant to go for it.

Is there any effect of TIG nozzle sizes, Moisture condensation at regulators?.

Some of the Pipes are received from China, is there any material chance?.

This problem typically we obseve in 6" & 8" Pipes.

Your suggestions noted, i will work on those.

Thank you for your valuable suggestions.

regards

P.Rao.

+968 93883351



On Friday, 14 February 2014 7:57 AM, pgoswami <pgoswami@quickclic.net> wrote:
Hi Mr.. Rao,
 
These black spots are essentially the products of contamination in the weld metal.There may not be a single reason towards this .It may happen as follows:-
  • Welding Fillers :- The drawing lubricants e.g graphite could contaminate the welds and cause  these spots to be formed. Through acetone cleaning of all the fillers should be done before welding. Also fillers with oxidized tips should be used following  removal of the oxidized tip(by cutting).
 
  • Shielding gas: check the purity of the gas, it should be 99.95% or more.  Premixed gases say Ar+N2 may contain traces of moisture , which  may increase the oxygen potential and the resultant oxidation of the puddle. As you said  earlier the "O2" content was  well below 0.2%.. Assuming the fact that  for shielding gas everything was under control it would be always advisable to check the right purity of the shielding and purging gas, prior to welding.
 
  • The condition of the pipes:- Duplex pipes should always be pickled  and cleaned at the mill. If not done at the mill, it's preferred to pickle the pipes and remove the excess scale or oxides in the fabrication shop. Usually such oxides could be very microscopic and very difficult to remove by grinding. Excess oxides may introduce contamination in the weld.Also cross contamination during grinding could harm the welds.
 
The dark spots are bad , with potential for pitting during procedure qualification testing or while put in service.
 
Let me know if it helps.
 
Thanks
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
 


From: Vasantharao [mailto:vasantharao@yahoo.in]
Sent: Wednesday, February 12, 2014 11:57 PM
To: pgoswami
Subject: Fw: Black spots on DSS Weld Joints.


Dear sir,

Can you give you suggestions on DSS dark spots as group member are not responding.

Is there any problem with dark spots. Why it forms. 

regards
P.Rao

On Wednesday, 12 February 2014 1:38 PM, Vasantharao <vasantharao@yahoo.in> wrote:
Dear Experts,

We observe Dark spots on Welding of Duplex Stainless Welds.  

Material is : UNS S31803 ,  Filler Wire for root - ER2594, rest ER2209.

Sample pictures are attached for reference.

Oxygen level in shielding / Purging maintained well below 0.2%.

Interpass <150 Deg.C

Pl. share your valuable information.

Thank you.

P.Rao


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...