Re: [MW:18000] Cracks on Hard Facing Overlay

Dear Sevak:



Check-cracking, or checking as it's sometimes called, occurs in the metal carbide families and can be seen as cracks that are perpendicular to the bead length. They generally occur from 3/8 to 2 inches apart and are the result of high residual stresses of hard-facing weld metal as it cools. Other alloys such as the austenitic and martensitic families, don't crack when applied with proper welding procedures but for many of chromium carbide alloys, check-cracks appear when cooled to moderate temperatures; this is normal.

Again, be careful if you try to stop this cracks, the residual stress will build-up and whatever you do, it will eventually crack, this time it will be a wide long crack that tears your work-piece apart...!!!

Check cracks propagate through the thickness of the weld bead and stop at the parent metal, as long as it's not brittle (like your case). In cases in which the parent metal is hard or brittle, you should select a buffer layer of a softer, tougher weld metal. Like what Mr. Swamy recommended, Ni-base or austenitic buffer family are good choices for a buffer deposit.

Regards
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.kondori@petroyada.com
+98-2123592322
+98-9132150320



On Sat, Jun 22, 2013 at 8:25 AM, pgoswami <pgoswami@quickclic.net> wrote:
Hello Hiren,
 
Hard facing alloys usually have little or low ductility as compared to many other corrosion or erosion resistant alloys. However cracks are not accepted as a rule. Hard facing containing cracks could be dislodged in service, if the extent of cracking is severe.
 
Perhaps adjusting the composition would be the way to go. The other technique could be use of austenitic(Ni based ) barrier layer.
 
What' re the technical requirements ?? You refer this article for general guidance.
 
Thanks.
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
 
http://www.twi.co.uk/news-events/bulletin/archive/pre-1998-articles/1991-articles/cracking-of-hardfacing-alloys-prevent-cure-or-ignore/

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of cbe swamy
Sent: Friday, June 21, 2013 1:30 AM
To: materials-welding@googlegroups.com
Subject: RE: [MW:17993] Cracks on Hard Facing Overlay

Dear All,
Where direct fusion welding is not appropriate, as in the case of an extremely hot-crack-sensitive casting, other
approaches might prove useful. One option is to "

Date: Fri, 21 Jun 2013 09:49:43 +0530
Subject: [MW:17992] Cracks on Hard Facing Overlay
From: hirensevak80@gmail.com
To: materials-welding@googlegroups.com

Dear Experts,
 
One of the manufacturer is using XL-CCH electrodes for Hard Facing Weld Overlay on c arbon steel material. (Chromium Carbide Alloy Deposit Hard Facing Electrode).
 
The weld overlay outer surface is showing parallel hair line cracks.
 
The manufacturer is arguing that these cracks are bound to develope due to inherrent properties of electrode & it is good to observe cracks on weld for ensuring the application of these type of electrode. The electrode catalogue also states that cracks can be developed on weld surface.
 
My question is which code/standard allow cracks on such hard facing overlay ?
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...