Tuesday, April 9, 2013

Re: [MW:17324] RE: 17307] Fwd: hardness limit for SA 516 Gr. 70

Hi maximum 200 HV , say me the thickness? If is more tha 19 mm need PWHT, is less 19 mm is probably very bad welding procedure in both case check WPS and PQR.

Agustin
Enviado desde mi BlackBerry de Movistar

From: "pgoswami" <pgoswami@quickclic.net>
Sender: materials-welding@googlegroups.com
Date: Tue, 9 Apr 2013 08:19:49 -0400
To: <materials-welding@googlegroups.com>
ReplyTo: materials-welding@googlegroups.com
Subject: RE: [MW:17323] RE: 17307] Fwd: hardness limit for SA 516 Gr. 70

Manoj,
 
As pointed out by John Henning, this hardness value of 340 HV is extremely high for SA 516/70 steel welds.Typically where hardness restriction is imposed,PWHT is mandatory.
 
What're  the design conditions, process fluid, to be handled.
 
Generally for -40 Deg design conditions PWHT should be mandatory as PWHT improves impacts, along with reduction of hardness.
 
Thanks
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of manoj john
Sent: Tuesday, April 09, 2013 6:28 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:17321] RE: 17307] Fwd: hardness limit for SA 516 Gr. 70

Dear Mr. John,
Thanks for your information.
According to your information i can use both the WPS, there will not be a code issue but i have to discuss with client.
With Regards,
Manoj


On Mon, Apr 8, 2013 at 6:53 PM, John Henning <jhenning@deltak.com> wrote:

This is not an ASME Code issue – Code does not require hardness testing.

 

This is a customer/client requirement and would need to be negotiated with him/her.  Note that 340HV10 (~322HBW) is a lot more than a little high.  The required hardness range and number of tests or number of separate PQRs is only a negotiation issue between you and them.  Without PWHT, hardness for carbon steel is directly related to heat input, welding sequence, etc. so hardness from one PQR may not be accepted for another PQR by your client unless there is substantial agreement in welding parameters.

 

There isn’t much help that can be given, I’m afraid.

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of manoj john
Sent: Monday, April 08, 2013 12:56 AM
To: materials-welding@googlegroups.com
Subject: [MW:17307] Fwd: hardness limit for SA 516 Gr. 70

 

Dear All,

 

Regarding the subject matter I need to clarify one more thing:

 

I have another WPS without hardness test as per ASME SEC. IX and with impact test, is it possible to use this procedure without hardness test,  all other variables are meeting the requirement or is it required to carry out hardness test for procedure qualification.

 

I have to carry out hardness test on the job.

 

Vessel Detail:

Vessel construction code is ASME SEC. VIII Div 1 Ed. 2010.

MOC : SA 516 Gr 70.

Shell / Dished end thickness : 22 mm/ 28 MM

Welding process : SMAW.

Heat treatment : NIL

Impact test : Required at minus 40 degree centigrade.

as per project spec. hardness to be checked and reported.

 

Welding procedure qualification details:

 

WPS No.  1 :   Material  : SA 516 GR 70.

                       Thickness range qualified  : 16 mm to 50 mm (test coupon 25mm)

                       Welding process : SMAW

                       Electrode : E 7018-1

                       Qualification position  : 3G

                       Preheating  : 40 degree centigrade

                       Impact tested at minus 46 degree centigrade.

                       Heat treatment : Nil

                       Hardness test : 340  HV10

 

WPS No.  2 :   Material  : SA 516 GR 70.

                       Thickness range qualified  : 16 mm to 36 mm (test coupon 18mm)

                       Welding process : SMAW

                       Electrode : E 7018-1

                       Qualification position  : 3G

                       Preheating  : 40 degree centigrade

                       Impact tested at minus 42 degree centigrade.

                       Heat treatment : Nil

                       Hardness test : not carried out.

 

Please give expert opinion.

 

Thanks and Regards.

 

On Sun, Apr 7, 2013 at 6:03 PM, manoj john <manojacgnr@gmail.com> wrote:

Dear members,

 

I have one pressure  vessel to fabricate as per ASME Sec. VIII Div.  1  Ed. 2010.  Client need hardness test and impact test requirement.

 

My doubt is that -   Is it required the hardness test for welding procedure qualification test because I already have one qualified procedure as per ASME SEC IX with hardness and impact test but the hardness is on little higher side (HV10 340)

 

Please clear my doubt.

 

Thanks in advance 

 

Manoj.

 

 

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 