Hi Aly ,
 
Attached please find  some very relevant information on SAW wire and flux combinations guaranteed  for good impact down up to  -46 Deg C. If  both impact and sour service hardness requirements are involved then EM12K would be the  "most preferred option". However  for this wire advise  would be to get a  weld metal composition  so as to get "Mn" around 1.2% max.
 
Higher "Mn" SAW wires e.g EH12K is good to guarantee  the UTS and impact  after PWHT , however meeting NACE hardness could be a problem. If the material to be welded is SA 516/70, there should not be many issues, however  while welding thicker sections of SA 537Cl1, EM12K sometimes may under match the UTS.
 
It would be advisable to get consumable manufacturer's  recommendations meeting all the technical requirements.
 
I hope this would help  you.
 
Keep posted.
 
Regards
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Aly
Sent: Wednesday, April 10, 2013 12:25 PM
To: materials-welding@googlegroups.com
Subject: [MW:17336] Request to provide filler metal & Flux combination for SAW process for low temperature service with Heat treatment

Dear Experts,

We are going to qualify welding procedure of following details

 

1.       Welding with

·         GTAW with ER70S2

·         SMAW with E7018-1 &

·         SAW

 

2.    Heat treatment after welding at 620°C @ 200min

3.    Impact testing after heat treatment at -46°C

 

Kindly  advise on  filler metal & Flux combination for SAW process to achieve impact properties after heat treatment.

 

Can F7A8 EM12K  will this serve the purpose…!!

 

 

Thanks & regards

 

Ali Mhaskar,

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...