Re: [MW:16686] PWHT Temperature for welding CS To SS

Dear Sevak,

As per ASME B 31.3,

331.2.3 Dissimilar Materials
(a) Heat treatment of welded joints between dissimilar
ferritic metals or between ferritic metals using dissimilar
ferritic filler metal shall be at the higher of the
temperature ranges in Table 331.1.1 for the materials in
the joint.
(b) Heat treatment of welded joints including both
ferritic and austenitic components and filler metals shall
be as required for the ferritic material or materials unless
otherwise specified in the engineering design.


Regards,
Santosh.

On Fri, Jan 25, 2013 at 8:08 AM, Prakash Hegde <pb.hegde@yahoo.com> wrote:
Controlling factor for PWHT temp  is CS and not SS  and we have heat treat as per ASME code UCS 56 or any applicable code
 
Regards
 
Hegde Prakash
----- Original Message -----
From: sevak hiren <hirensevak80@gmail.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Cc:
Sent: Thursday, 24 January 2013 12:04 PM
Subject: [MW:16587] PWHT Temperature for welding CS To SS

Dear Experts,

Kindly suggest what should be the PWHT Temperature after welding of
following dissimilar materials.

SA 516 Gr.70 To SA 240 Gr.304

Regards

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...