Wednesday, September 12, 2012

RE: [MW:15287] RE: 15280] Welder Qualification Range for CS to alloy with same dia and thickness?

If you have a qualified wps with A335 P9  do it, but  performance test internally is better.
 
Regards

QW-433 Alternate F-Numbers for Welder Performance Qualification


The following tables identify the filler metal or electrode that the welder used during qualification testing as "Qualified


With," and the electrodes or filler metals that the welder is qualified to use in production welding as "Qualified For."


See table QW-432 for the F-Number assignments

Qualified With

 

 


 

Qualified With Qualified For

Any F-No. 6 All F-No. 6 [Note (1)]

Any F-No. 21 through F-No. 25 All F-No. 21 through F-No. 25

Any F-No. 31, F-No. 32, Only the same F-Number as was

F-No. 33, F-No. 35, F-No. 36, used during the qualification

or F-No. 37 test

F-No. 34 or any F-No. 41 F-No. 34 and all F-No. 41

through F-No. 46 through F-No. 46

Any F-No. 51 through F-No. 55 All F-No. 51 through F-No. 55

Any F-No. 61 All F-No. 61

Any F-No. 71 through F-No. 72 Only the same F-Number as was

used during the qualification

test

NOTE:

(1) Deposited weld metal made using a bare rod not covered by an SFA

Specification but which conforms to an analysis listed in QW-442

shall be considered to be classified as F-No. 6.

143


 

 

 

 


Subject: [MW:15283] RE: 15280] Welder Qualification Range for CS to alloy with same dia and thickness?
Date: Wed, 12 Sep 2012 11:08:51 -0500
From: jhenning@deltak.com
To: materials-welding@googlegroups.com

yes

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Biplab Pal
Sent: Wednesday, September 12, 2012 7:42 AM
To: materials-welding
Subject: [MW:15280] Welder Qualification Range for CS to alloy with same dia and thickness?

 

Dear Experts,

 

1 welder is qualified with ASTM A 106 Gr. B with ER70S-6 (Root & 2nd Pass) & E7018(Fill & Cap) with a diameter range of 2 7/8 and above

If thickness and dia of pipe remain same, can he weld on ASTM A 335 Gr. P-9 with ER80s B8 & E 8018 B8.

Construction Code Sec-IX, 2010.

--
Thanks & Regards
Biplab Pal
Mechanical Inspector (PMT)
E-mail:   biplab.mech@gmail.com
 
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...