Dear Arun, 

 

In my previous mail, I have mentioned as, "Only Heat input shall be controlled during test coupon welding and H.I values shall not exceeds the previous qualified PQR value and other essential shall be as per previous qualified PQR", this means I have suggested Mr. Mubben even not to make any changes in supplementary variable during additional coupon welding.

 

Now coming to ASME SEC 09 QW 200.1.C, it states   "Changes in essential or supplementary essential (when required) variables require requalification of the WPS (new or additional PQRs to support the change in essential or supplementary essential variables)."

 

If heat input values are higher than previous qualified PQR, supplementary essential variable shall be an essential variable as per QW 252 through QW 266. In Mr. Mubeen case only Additional PQR by conducting impact test at -46 Deg C will be suffient.

 

As a good engineering practice to achieve good Impact test results, maximum heat input values should be kept as low as possible.

 

Some clients in oil and gas industries does not allows heat input for Production joint  above  the range qualified in PQR ,when Impact and Sour service requirements are applicable.

 

Hope you understood.

 

 

With regards,

Sudhakar.K





On Mon, Sep 3, 2012 at 11:49 AM, sudhakar kuppuswamy <mechsudhakar@gmail.com> wrote:

 

Dear Mubeen,

 

No need to REDO the entire test.

 

You can weld a test coupon by using the existing WPS and only Impact test shall be carried out at -46 deg C.

 

 

Heat input shall be controlled during test coupon welding and H.I values shall not exceeds the previous qualified PQR value and ensure other essential shall be as per previous qualified PQR.

 

As per ASME SEC 09 clauses /tables from QW 252 through QW 266, increase in heat input is a supplementary essential variable. This refers to QW 409.1.


please refer to the above mentioned  clause in  ASME SEC 09.


 

Regards,

Sudhakar.K





On Mon, Sep 3, 2012 at 6:33 AM, mubeen mubeen <mubeenaws@gmail.com> wrote:
Dear experts, 

Please help out to clear my doubt. 

I have qualified a WPS/PQR with impact -29 deg C, now customer want the WPS/PQR shall be qualified with impact in -46 deg C. Also there is no remaining coupon piece available for impact testing with -46 deg C. 

My question here is, should I weld a coupon and only do impact test as required by customer and attached to PQR will be sort out this issue.? 
or 
Should I REDO a PQR with all mechanical  test which includes Tensile, Hardness, Bend along with impact will sort our this issue.? 


Requesting you to please provide me ASME IX clause reference.


Anticipating for you kind help. 

Thanks & Regards. 
M.K.Mubeen

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...