Saturday, December 31, 2011

Re: [MW:13374] Failure Of Root bend test of Welding (CS to SS)

Dear HAREESH,
What was the welding position? If It was not 1G or 2G which on of the root samples failed (acc. to he test sketch in ASME Sec. IX)?
 
Regards

On Sat, Dec 31, 2011 at 8:35 AM, HAREESH K V <hareesh13h@gmail.com> wrote:
Dear Sir,
 
Advance happy new year to all.
 
I have done a PQR(As per ASME Sec ix) of 6", Sa106 GrB to Sa 312 TP 316L. One of the root bend of the same failed.
 
Consumable used: ErNiCr-3. 
 
Tesile strength T1=507 and T2=514MPa(Min Rqd 415MPa);
 
Hardness:
Sa106 Gr B side p.metal: 160,151,147
Sa106 Gr B side HAZ:160,156,156
Weld: 193,170,165
Sa312 TP316L P.metal: 175, 175,181
Sa312 TP316L HAZ: 165,151,151
Face bends are satisfactory.
 
One root bend satisfactory.
 
Please give me the possible reasons and the precautions on further doing the PQR.
 
Regards,
 
Hareesh K V

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
M. Shokri Arfaei
International Welding Engineer (IWE)
ASNT NDT Level III
ERI Metallurgy Lab. Manager
Tel: +98-21-66282127
Fax: +98-21-66282779
 
Please don't print this e-mail unless you really need to. BeGreen!

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...