Re: [MW:13334] REGARDING Impact test of VESSEL PRODUCTION TEST COUPON

Dear Vivek,
                70% of required average is ok, ur values r ok to pass the PTC.

2011/12/27 Vivek Pandey <vivek.pande06@gmail.com>
Respected All,


I want your suggestion about Impact test of vessel production test, I
have tested a stress relieved PTC Impact test on weld & HAZ AT -47
DEG. PTC has failed again I have  done  reheat treatment & Retest with
same cycle of the job. PTC has failed in one indivzual value by 1
joule.Value is like this way 28, 19, 34.


Is there any acceptance criteria as per ASME SECTION VIII DIV 1. other
wise all weld of category A B C D to be gauged & reweld.

Kindly solve my query as soon as possible



Regards
VIVEK PANDEY

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
regards,
Harish.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...