Dear all,

 

As far as I know Sa2,5  indicates the surface cleaness (the rust grade) of the substrate see ISO 8501). Surface roughness calues can be estimated using surface profile comparators (e.g  see  EN ISO 8503)

 

Regards

 

S. Akyuz

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Pieper QSI
Sent: Friday, December 23, 2011 12:08 PM
To: materials-welding@googlegroups.com
Subject: RE: [MW:13277] Surface roughness measurement instruments.

 

Dear Mr. Rao,

 

Be aware that the microns you mention is not the surface roughness but the coating layer thickness (DFT = Drie Film Thickness).

For surface roughness you will have values like SA 2,5 microns or similar and in practice mostly the comparators are used for inspection prior to first layer of coating.

After fist coating layer there is no need to measure the roughness anymore.

 

Met vriendelijke groeten / Best Regards

 

Herman Pieper

 

Pieper Quality Support & Inspection

Phone: +31 (0)521 380083

Fax:     +31 (0)84 7539225

Cell:     +31 (0)6 51691215

www.pieper-qsi.nl

 

Van: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Namens jsrisud@gmail.com
Verzonden: donderdag 22 december 2011 14:45
Aan: materials-welding@googlegroups.com
Onderwerp: Re: [MW:13259] Surface roughness measurement instruments.

 

Dear Mr. Rao,

There are portable surface roughness measuring instruments to measure as required.

UK based Rank Taylor Hobson instruments are available in India.

Srinivasan

Sent from BlackBerry® on Airtel


From: Vasantharao <vasantharao@yahoo.in>

Date: Thu, 22 Dec 2011 15:38:40 +0530 (IST)

Subject: [MW:13256] Surface roughness measurement instruments.

 

Dear Experts,

 

I work as inspection Engineer. When i go for Blasting inspection, contractor provided  me profile comparator for surface roughness measurement.

 

Contractor do  Grit blasting in the shop.

 

I need to measure surface roughness  -  75-100 microns      Painting system No#1

                                                            50-75 microns        Painting system No#2

Queries

Q 1: Comparator is enough for surface roughness measurements.

 

Q2: Is any other tools available for roughness measurement?.

 

Q3:  What is the normal industry practice.


Pl. provide your valuable suggestions as i'm new for painting activities.

Rao.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...