Re: [MW:12676] need to add a pipe to a piping station, do we need to make hydrostatic test again?

Dear tugrulhan özdemir,


Just make a fabrication, and do the 100% radiography of joints its according to Chinese standard. If your client is not satisfied  then you have a Leak test option.
but leak test + 100% radiography.

***************************************************

On Fri, Oct 14, 2011 at 9:06 PM, Umut Cahit Akbay <umutcahit@gmail.com> wrote:
Depending on the wall thickness and the service of the line (potable water I assume), you can make %100 percent X-ray or UT (and also in order to convince the client, bubble test priour to the painting activities) as per ASME B31.3 Process Piping.
Quoting from the 2006 edition of the abovementioned standard:

"345.9 Alternative Leak Test
The following procedures and leak test method may
be used only under the conditions stated in para.
345.1(c).
345.9.1 Examination of Welds. Welds, including
those used in the manufacture of welded pipe and fittings,
which have not been subjected to hydrostatic or
pneumatic leak tests in accordance with this Code, shall
be examined as follows:
79
(a) Circumferential, longitudinal, and spiral groove
welds shall be 100% radiographed in accordance with
para. 344.5 or 100% ultrasonically examined in accordance
with para. 344.6.
(b) All welds, including structural attachment welds,
not covered in (a) above, shall be examined using the
liquid penetrant method (para. 344.4) or, for magnetic
materials, the magnetic particle method (para. 344.3)."

Be sure that client like aramco and SWCC will be hard to deal with, you need to convince them properly.


2011/10/14 tugrulhan özdemir <tugrulhan9@gmail.com>

Dear Welding People



I have 1 question for you


We had finished the hydrotesting of the pump station. But now electric
company ask for adding 1 pipe (2 inch)  to a 40" pipe. But we have
already finished the hydrotest for this line. I need to know does
anyone know any standard or specification that tells any solution for
this sitaution except re-hydortesting.



Thanks for kind attention

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Umut C. AKBAY

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Regards,

Jawad Hanif
Mechanical Engineer

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35289] Welding consumable for S355J2WP material

S355 J2 WP  is a weathering structural steel  It has better atmospheric corrosion resistance. Use E 8018 - W1/W2  Electrodes This is regular...