Hi,
In this case you may have to use solid titanium material or exploasion bonded clad sheet.
Thanks & Regards
Muhammed Ibrahim PK
On 17 June 2010 20:34, Shadab Ansari <shadabansarialam@gmail.com> wrote:
Dear Mr. Ibrahim,What if the corrosion resistant material is Titanium which cannot be easily overlaid over CS material?Regards
Shadab Alam Ansari
Welding Engineer
Olayan Descon
On Thu, Jun 17, 2010 at 7:01 AM, Muhammed Ibrahim PK <ibratech@gmail.com> wrote:Dear Shadab,The tube sheet thickness shall be same as job thickness except it does not required more than 50 mm.In your case you can make a test coupon with 50 mm thick+Weld overlay 10mm.There are many essentila variables. Refer QW-193, QW-288. in ASME Sec IX.Regards,IbrahimOn 16 June 2010 23:14, Shadab Alam Ansari (Welding Engineer) <shadabansarialam@gmail.com> wrote:What should be the range of the Tube sheet thickness minimum and
maximum qualification as per Sec-IX?
Also if i have a corrosion resistant overlay of 10mm on 120mm base
metal, can we use the Corrosion resistant material as a base metal of
same 10 mm thickness for making tube to tube sheet weld joint?
Regards
Shadab Alam Ansari
Welding Engineer
Olayan Descon
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
Thanks & Regards
Muhammed Ibrahim PK--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
No comments:
Post a Comment