Thursday, June 17, 2010

Re: [MW:5633] RE: 5612] Barrier layer for corrosion resistant overlay

Dear All,
 
Finally, Valve manufacturer is agree to do the barrier layer by E-309.
 
Thanks,
 
Regards,
 
atul

 
On Wed, Jun 16, 2010 at 2:57 PM, Prabhu Kumar L <l.prabhukumar@saipem-india.com> wrote:

Dear Mr. Dilintas,

 

Please note that Austenitic SS electrodes such as E/ER316, E/ER308 is having ferrite content of around 9 to 10% would sufficient to avoid hot cracking. In case of 309 type, the % of ferrite is around 15 to 20%.

 

According to schaffler diagram, if we use 316/308 type electrodes directly on CS/LAS, the microstructure in the fusion line may fall in the Austenite + Ferrite + Martensite zone, since dilution of 30 to 35% would take place in the zone. However, the end micro-structure is supposed to be Austenite+ Ferrite.

 

Hope it clarifies.

 

Regards,

 

L. Prabhu kumar,

Sr. Principal Engineer,

 

Equipments & Materials Dept.,

Saipem India Projects Limited,

Nungambakkam High Road, Chennai - 600 034, India.

Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,

Mobile Ph. No.: +91 9003010978.


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of george.dilintas@gr.bureauveritas.com
Sent: Wednesday, June 16, 2010 3:51 PM

Subject: Re: [MW:5615] RE: 5612] Barrier layer for corrosion resistant overlay

 

Yes but the purpose of the barrier with E309 is to avoid hot cracking due to low FN and not martensite formation

Dr. G. Dilintas - Authorized Inspector Supervisor
I&F Regional Technical Manager
Bureau Veritas Piraeus - Greece
Tel: +30 210 40 63 113/4
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04
Inactive hide details for "Prabhu Kumar L" <l.prabhukumar@saipem-india.com>"Prabhu Kumar L" <l.prabhukumar@saipem-india.com>

"Prabhu Kumar L" <l.prabhukumar@saipem-india.com>
Sent by: materials-welding@googlegroups.com

16/06/2010 12:31

Please respond to
materials-welding@googlegroups.com

To


<materials-welding@googlegroups.com>

cc

Subject


[MW:0] RE: 5612] Barrier layer for corrosion resistant overlay

Ref

 


Dear Mr. Atul,

As you mentioned, in general most of value manufacturers carryout
overlay on seating area with direct matching electrodes (E316) without
using barrier layer electrodes i.e. with E309 type due to the following
reasons.

- Overlay on seating area is not for corrosion purpose. It is required
for purpose of wear resistance to contact with the matching part.
- Most of the manufacturers are using automatic welding system to
carryout this overlay, hence the dilution problems are minimized.

If it is applicable for corrosion resistance purpose, it is strongly
recommended to use high alloyed electrodes for barrier layer (E309) and
rest by the matching electrodes in order to minimize dilution and
avoiding martensite formation in the interface, which will reduce the
corrosion properties.

Regards,

L. Prabhu kumar,
Sr. Principal Engineer,

Equipments & Materials Dept.,
Saipem India Projects Limited,
Nungambakkam High Road, Chennai - 600 034, India.
Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,
Mobile Ph. No.: +91 9003010978.

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of atul chaturvedi
Sent: Wednesday, June 16, 2010 1:41 PM
To: Materials & Welding
Subject: [MW:5612] Barrier layer for corrosion resistant overlay

Dear All,

I have a doubt regarding body seat corrosion resistant overlay welding
on valves by valve manufacturers .Can they use E316-16 directly on
body seat(A 216 WCB) without using dissimilar weld metal  barrier
layer

regards

atul

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.


-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or

entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged

information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution

or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If

you have received this communication in error, please notify us immediately by responding to this email and then

delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete

transmission of the information contained in this communication nor for any delay in its receipt.
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...