Skip to main content

RE: [MW:5622] RE: 5612] Barrier layer for corrosion resistant overlay

Dear Mr. Dilintas,

 

Please note that Austenitic SS electrodes such as E/ER316, E/ER308 is having ferrite content of around 9 to 10% would sufficient to avoid hot cracking. In case of 309 type, the % of ferrite is around 15 to 20%.

 

According to schaffler diagram, if we use 316/308 type electrodes directly on CS/LAS, the microstructure in the fusion line may fall in the Austenite + Ferrite + Martensite zone, since dilution of 30 to 35% would take place in the zone. However, the end micro-structure is supposed to be Austenite+ Ferrite.

 

Hope it clarifies.

 

Regards,

 

L. Prabhu kumar,

Sr. Principal Engineer,

 

Equipments & Materials Dept.,

Saipem India Projects Limited,

Nungambakkam High Road, Chennai - 600 034, India.

Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,

Mobile Ph. No.: +91 9003010978.


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of george.dilintas@gr.bureauveritas.com
Sent: Wednesday, June 16, 2010 3:51 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:5615] RE: 5612] Barrier layer for corrosion resistant overlay

 

Yes but the purpose of the barrier with E309 is to avoid hot cracking due to low FN and not martensite formation

Dr. G. Dilintas - Authorized Inspector Supervisor
I&F Regional Technical Manager
Bureau Veritas Piraeus - Greece
Tel: +30 210 40 63 113/4
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04
Inactive hide details for "Prabhu Kumar L" <l.prabhukumar@saipem-india.com>"Prabhu Kumar L" <l.prabhukumar@saipem-india.com>

"Prabhu Kumar L" <l.prabhukumar@saipem-india.com>
Sent by: materials-welding@googlegroups.com

16/06/2010 12:31

Please respond to
materials-welding@googlegroups.com

To


<materials-welding@googlegroups.com>

cc

Subject


[MW:0] RE: 5612] Barrier layer for corrosion resistant overlay

Ref

 


Dear Mr. Atul,

As you mentioned, in general most of value manufacturers carryout
overlay on seating area with direct matching electrodes (E316) without
using barrier layer electrodes i.e. with E309 type due to the following
reasons.

- Overlay on seating area is not for corrosion purpose. It is required
for purpose of wear resistance to contact with the matching part.
- Most of the manufacturers are using automatic welding system to
carryout this overlay, hence the dilution problems are minimized.

If it is applicable for corrosion resistance purpose, it is strongly
recommended to use high alloyed electrodes for barrier layer (E309) and
rest by the matching electrodes in order to minimize dilution and
avoiding martensite formation in the interface, which will reduce the
corrosion properties.

Regards,

L. Prabhu kumar,
Sr. Principal Engineer,

Equipments & Materials Dept.,
Saipem India Projects Limited,
Nungambakkam High Road, Chennai - 600 034, India.
Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,
Mobile Ph. No.: +91 9003010978.

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of atul chaturvedi
Sent: Wednesday, June 16, 2010 1:41 PM
To: Materials & Welding
Subject: [MW:5612] Barrier layer for corrosion resistant overlay

Dear All,

I have a doubt regarding body seat corrosion resistant overlay welding
on valves by valve manufacturers .Can they use E316-16 directly on
body seat(A 216 WCB) without using dissimilar weld metal  barrier
layer

regards

atul

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.


-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or

entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged

information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution

or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If

you have received this communication in error, please notify us immediately by responding to this email and then

delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete

transmission of the information contained in this communication nor for any delay in its receipt.
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


 

 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...