Hi MOHAMMED too you can use Root pass with E7010A1 and rest by E8018G by uphill progression, We welded with it welding procedure.
the 7018 stress is very close the base metal stress, is better use 8018.
 
Agustin



De: Prabhu Kumar L <l.prabhukumar@saipem-india.com>
Para: materials-welding@googlegroups.com
Enviado: mar, junio 8, 2010 3:37:30 AM
Asunto: [MW:5463] RE: 5437] welding Pipe API 5LX52 to Flange ASTM A105

Dear Mohammed,

 

You can follow any one of the option for welding of X52 to A105.

 

  1. Root pass with E6010 and rest by E7010 by uphill or dollymix (root-uphill and rest-downhill) progression.
  2. Root pass with E6010 and rest by E7018 by uphill progression

 

No restriction on use of cellulosic or low hydrogen electrodes for welding of pipe to fittings/ flanges. However, for any repair welding, it is recommended to use low hydrogen electrodes in order to reduce hydrogen induced cracking problems.

 

Regards,

 

L. Prabhu kumar,

Sr. Principal Engineer,

 

Equipments & Materials Dept.,

Saipem India Projects Limited,

Nungambakkam High Road, Chennai - 600 034, India .

Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,

Mobile Ph. No.: +91 9003010978.


From: materials-welding@googlegroups.com [mailto: materials-welding@googlegroups.com ] On Behalf Of mohammed helal
Sent: Monday, June 07, 2010 11:09 PM
To: materials-welding@googlegroups.com
Subject: [MW:5437] welding Pipe API 5LX52 to Flange ASTM A105

 

For welding Pipe API 5LX52 to Flange ASTM A105  in a pipe line project we should use 7018 or 7010 is enough to give us the desired quality.( i think that fitting to fitting we have use 7018 but fitting to pipe, can we use 7010)

Eng.MOHAMMED ABD EL-AZIM HILAL

        MECHANICAL ENGINEER

     CSWIP 3.1 - NDT (RT- MT - PT)

OTISHAN CONSULTANT ENGINEER

 00966-502612218  -  0020103124557

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

 




-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or 
entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged 
information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution 
or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If 
you have received this communication in error, please notify us immediately by responding to this email and then 
delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete 
transmission of the information contained in this communication nor for any delay in its receipt. 
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...