Hi.
cover and Preheat at 350 oF minimun and let cool very slowly, rate 50 oF per hour, used heat treating machine for major parameter control.
 
Agustin


De: Jimmy Nielsen <nielsen.jimmy@gmail.com>
Para: materials-welding@googlegroups.com
Enviado: mar, junio 8, 2010 3:04:45 AM
Asunto: Re: [MW:5460] How to control the hardness in P22

Cover the weld with insulation and let it cool slowly.

Regards, jimmy

On 8 Jun 2010 14:02, "mahendran p" <pmahe_79@yahoo.co.in> wrote:
> Hi all,
>          May any one tell me, how to control the hardness of the P22 materials welding without PWHT. Even, we do pre-heating as per the ASME 31.3 & also we use 2.6mm dia electrode(E9016/8). Still we get the hardness around 290 HB.
>  
> Any suggestions to control the hardness within 241 HB(ASME 31.3).
>  
>  
> Please help.
> Thank you.
> Best regards,
> P.Mahendran
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...