Hi Prabhukumar,
                          I hope we need the match the weld metal since due to dilution during welding there will be further pick up of carbon in case of "L" or loss in case of Non" L".Also strength point of view it'l match .It's advised by API RP 598 also 

vaithiyanathan,
QA Engineer,
WorleyParsons Arabian Industries
Oman

On Thu, Jun 3, 2010 at 10:07 AM, Prabhu Kumar L <l.prabhukumar@saipem-india.com> wrote:

Hi Velomany,

 

First of all, I would like to know why do you want to use E/ER316 filler metal for cryogenic application. No restriction that base and filler metal should be same except if application is high temperature, which requires minimum of 0.04% carbon. It is suggested to use low carbon filler metal grades in order to achieve better toughness properties at lower temperatures.

 

I understand that the Client specification restricts only on base material for qualification purpose and not on filler material. You can use E/ER316L filler materials using SS316 base material for qualification. As per B31.3, cl. ref. 323.2.2 (f) (2) (a) and Table 323.2.2, toughness tests are required only for weld metal if MDMT is colder than -101 Deg. C. Also read note no. 2 of Table 323.2.2 for combining production weld test coupon requirements in order to meet the base metal thickness range as specified in Table 323.3.- A (5).

 

For cryogenic application, the deposited weld metal shall have 2-5% delta ferrite in order to meet the toughness at cryogenic temperature (-196 Deg. C). More than 5% would reduce toughness on weld metal (typically it should be 2-3%).

 

In recent past most of the manufacturers are producing duel grade materials that would meet requirements of both the grades such as SS316/316L. However, these materials cannot be used for critical applications such as cryogenic and high temperature etc, it can be used for general applications.

 

Hope it clarifies your query.

 

Regards,

 

L. Prabhu kumar,

Sr. Principal Engineer,

 

Equipments & Materials Dept.,

Saipem India Projects Limited,

Nungambakkam High Road, Chennai - 600 034, India.

Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,

Mobile Ph. No.: +91 9003010978.


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of veloumany siva
Sent: Wednesday, June 02, 2010 8:42 PM
To: materials-welding@googlegroups.com
Subject: [MW:5355] ER316 & E316-16 FOR CRYOGENIC SERVICE

 

Dear all,

 

 

one of our Client specification says"Qualification on Material Gr.316 also qualifies for Gr.316L but not Vice versa"

 

I want to esatblish WPS for Stainless steel Material Gr.316 (cryogrnic service) as per B31.3

 

 

My query is

 

whether  ER316 for GTAW Process and E316-16 for SMAW  will meet the Impact requirement?

 

 

Regards,

S.Veloumany

 

 

 

 

 



 

 




-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or 
entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged 
information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution 
or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If 
you have received this communication in error, please notify us immediately by responding to this email and then 
delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete 
transmission of the information contained in this communication nor for any delay in its receipt. 
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
With Best Regards

B.Vaithiyanathan

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...