Hi Pravan,
Duplex stainless steel can be overlayed on a substrate of C.S or LAS. Alternatively you may hard face on duplex S.S with due precaution because the interface would have a tendency to embrittle.
From your query I would presume that you want to overlay duplex S.S on a substrate of C.S or LAS. Under those circumstances the following would be be appropriate:-
- Barrier layer with E-309L/309LMo, use 1/8" diameter
- Subsequent layers with E-2209 , 1/8" OR 5/32" dia.
The barrier layer chemistry is greatly affected by the dilution rate which depends on the welding parameters. Hence choose the optimum welding parameters as per consumable manufacturer. The same applies for the subsequent layers also.
Follow the guidelines in ASME Sec-IX for qualification of welding procedures.
Thanks
Pradip Goswami,P.Eng
Welding & Metallurgical Engineer/Specialist
Ontario Power Generation Inc.
Temp Mobile No (In India till 16 March)-9830976290
> Date: Sun, 7 Mar 2010 03:36:14 +0200
> From: p_chavdarov@mail.bg
> To: materials-welding@googlegroups.com
> Subject: [MW:4457] hard-facing of duplex steels
>
> Dear colleagues,
>
> has somebody experience with overlaying of duplex stainless steel
> 2205? Can you send me some details regarding the fillers and the
> welding parameters or an example of a WPS?
>
> Preliminary thanks
> Parvan Chavdarov
>
> -------------------------------------
>
> Внимание! Разбрахте ли, че вече Webexpert е в BG
> Безплатен домейн, 50 GB място, 3 сайта на 1 хост,
> 24/7 Професионална поддръжка, Отдалечен Back-up
> http://webexpert.bg/
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
No comments:
Post a Comment