[MW:3634] Re: Xlyan Coating, Mud cracking appears on Well head casing

Though it has been several years since i lasted used Xylan coatings here
is what I remember:

Check the thickness of the Xylan Coating
The coating thickness should be in this range

Thickness .0008" - .002" (0.02032mm - 0.0508mm) any thicker and Mud
Cracking will readily occur.

Watch your application temperature , too high and solvent will evaporate
too fast causing a mud cracking even if in the correct thickness range.

Best regards,

Richard M. beldyk PhD, PE


Original Message:
-----------------
From: SENTHILKUMAR SWAMINATHAN skumarswami@yahoo.co.in
Date: Wed, 11 Nov 2009 14:55:14 +0530 (IST)
To: materials-welding@googlegroups.com
Subject: [MW:3633] Xlyan Coating, Mud cracking appears on Well head casing


Dear Experts,
 
In my Co Painting dept facing mud cracking after heat treatment in Xlyan
Coating. what needs to do in this sitiuation?
 
Thank you
Regards,
S.Senthilkumar
 


The INTERNET now has a personality. YOURS! See your Yahoo! Homepage.
http://in.yahoo.com/

--------------------------------------------------------------------
mail2web.com – Enhanced email for the mobile individual based on Microsoft®
Exchange - http://link.mail2web.com/Personal/EnhancedEmail

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

Re: [MW:35354] Cast-iron welding

1. Preheat joint area(other area, cover with mineral wool). 2. ENiCi or ENiFe-CI. 3. stringer bead. 4. peening is to be done on weldmetal im...