We had successfully achieved this requirement on 40mm thk. plate (SA 516 Gr.70) for Dis end  using following consumables.

1) Root + Second Pass - E 8018 G
2) Remaining Passes - F7P2EH14
3) After Back chipping (Other side) -F7P2EH14

Regards

Atul Chaturvedi

On Wed, May 16, 2012 at 7:40 AM, pgoswami <pgoswami@quickclic.net> wrote:
Hi Ansari,
 
Please see the earlier discussion on the similar topic posted in ther forum.
 
Note other than "Mn" SA 516/70 steel does not have any alloying element, which can improve the mechanical properties after normalizing.Hence welding consumable with alloying elements are always advisable
 
Thanks
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Prakash Hegde
Sent: Sunday, May 13, 2012 10:35 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:14257] RE: 14217] Flux-Electrode Combination required.

Generly Normalizing + SR of 7018 catagory weld will not give required UTS of SA516 Gr70  as it deteorates the value
Therefore It is recomeded E9018 with higher Mn for welding Gr70 CS which undegoes NR but However more than 50 thk weld  with more than 2hrs Soaking time of NR even E9018 is not suitable.In such case The D/E of Crown and petal construction is recomended (With B2 having Cr is not suitable for such NR condition)
Incase of SAW process there is no suitble wire and flux combination (Even EH14 is not good) some time you can try EA3 or EF3 (SAF 5.23) but not for higher thk 
To get good results you may high to make trials with NR time and temp
 
Regards
 
Hegde P.B.
08805593046

--- On Sun, 13/5/12, kannayeram gnanapandithan <kgpandithan@gmail.com> wrote:

From: kannayeram gnanapandithan <kgpandithan@gmail.com>
Subject: Re: [MW:14255] RE: 14217] Flux-Electrode Combination required.
To: materials-welding@googlegroups.com
Date: Sunday, 13 May, 2012, 6:55 PM

If weld is subjected to Normalizing and then Stress releiving, 7
serious electrode will not work out, after heat treatment strenght
will come below minimum requirements,
Pl go for 8serious loke 8018-G ( tenaloy 60/65) for SMAW and for SAW
go for alloy steel wire -B2
Pandithan
In-Charge/WT
Cethar Ltd

On 5/9/12, pgoswami <pgoswami@quickclic.net> wrote:
> Mr. Ansari,
>
> *   
>
>     What's the design code?
> *   
>
>     any impact test requirements
> *   
>
>     any hardness requirements?
>
>
> Appreciate your response.
>
> Thanks.
>
>
> Pradip Goswami,P.Eng.IWE
>
> Welding & Metallurgical Specialist
>
> Ontario, Canada.
>
> Email-pgoswami@sympatico.ca <blocked::mailto:Email-pgoswami@sympatico.ca> ,
>
> pgoswami@quickclic.net <blocked::mailto:pgoswami@quickclic.net>
>
>
>
>   _____
>
> From: materials-welding@googlegroups.com
> [mailto:materials-welding@googlegroups.com] On Behalf Of ansari intekhab
> alam
> Sent: Tuesday, May 08, 2012 6:25 AM
> To: materials-welding@googlegroups.com
> Subject: [MW:14217] Flux-Electrode Combination required.
>
>
> Dear Experts
> Hi ,
> further can anyone suggest me that the electrode for SMAW  and Electrode and
> flux wire combination for SAW Process.
> Details as are
> 1. Material - SA 516-70
> 2.Thickness-70 mm
> 3.Normalizing-  ( 920 Deg - 150 min )  +  Dress relieving ( 620 Deg - 350
> Minutes ).
> also please suggest that how we can choose the electrodes and fluxes for a
> particular weld by using ASME Section 2 Part C.
>
> -
> Regards
> Ansari Intekhab Alam
>
>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...