Hi, Ezzudine Must
you can not use mild steel to weld Dissimilar steels. crack!!!
You know Cast Iron is too difficult to be welded, so in this case, you have two choices.
1, cast iron electrode: ENi-C1
2, Nickel base material: ENiCrFe-3 (wire:ERNiCr-3)
Please find enclosed sheets.
any question, please contact me.
Roy from Boehler Welding
From: Maulik Thakkar
Sent: Thursday, May 03, 2012 3:15 AM
Subject: Re: [MW:14174] suitables electrode used for cast iron
Dear all,
I think the question is wrong. Panama chock always made by cast steel rather by cast iron!!
Please understand difference between cast steel and cast iron!!!
Dear huzaifa please check your material of panama chock again
Regards,
Maulik Thakkar
Welding Engineer
L & T limited, Hazira
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
I think the question is wrong. Panama chock always made by cast steel rather by cast iron!!
Please understand difference between cast steel and cast iron!!!
Dear huzaifa please check your material of panama chock again
Regards,
Maulik Thakkar
Welding Engineer
L & T limited, Hazira
On Thu, Apr 19, 2012 at 2:02 PM, Karthik <karthik6684@yahoo.com> wrote:
--Hi,Please find herewith the attached file might be useful to you. You should use NiFe based electrodes for SMAW welding (AWS A5.15 ENiFe-CI)Thanks & Regards,(Karthik)Karthikeyan.SQA/QC ManagerGerman-Thai Boiler Engineering Cooperation Limited.Rayong Factory ;379 Moo.6 Soi 8, Tambol Pananikom,Nikompattana, Rayong 21180 THAILANDTel : +66 38 897 035-9 Ext. 137Fax : +66 38 897 034Hand Phone: 0066 892512282
From: Engr huzaifa shabbir <engr.huzaifa@gmail.com>
To: materials-welding@googlegroups.com
Sent: Thursday, April 19, 2012 1:38 PM
Subject: Re: [MW:14127] suitables electrode used for cast ironDEAR FRIEND,
IF YOU USED LOW HYDROGEN ELECTRODE FOR CAST FE 7& HIGH STRENGTH MATERIAL, THE WELD WILL CRACK OR MAY CRACK IN FUTURE
THE MOST SUITABLE ELECTRODE FOR THIS TYPE OF JOINTS IS ANY HIGH PERCENT NICKEL ELECTRODE.
FOR ANY QUERY U MAY CALL +923312041785
OR CONTACT ON engr.huzaifa@gmail.com
REGARDS
HUZAIFA
QA/QC ENGR
PEOPLE STEEL MILLS KHI
On Tue, Apr 17, 2012 at 2:39 PM, izzuddin mustafa <ezzudine@yahoo.com> wrote:
--
Hi experts,
I need your help. I prepared procedure to welding panama chock (cast iron material) to high tensile strength plate (EH 36). what is the suitable eloctrode to used for smaw process? can i used the ordinary low hidrogen eloctrode such as KOBE brand E 7018? or special elctrode? please advice me.
Thank you.
Ezzudine Must.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to mailto:materials-welding%2Bunsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to mailto:materials-welding%2Bunsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to mailto:materials-welding%2Bunsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
No comments:
Post a Comment