Skip to main content

Re: [MW:33863] Weld overlay PQR UNS 31254 (P8 Gr 4) To overlay SA516 GR70 overlay by ER Ni Cr MO-3

Regarding PQR Qualification,

Weld a clad plate of similar composition (as production Joint) with 254 SMO Alloy plate (based on production joint dissimilar thickness allowed)

Thanks & Regards

J.Gerald Jayakumar




On Monday, 26 December, 2022 at 08:40:51 am IST, 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> wrote:


Weld the joint as per attached configuration as a single vee joint using alloy filler wire/electrode such as ER/E NiCrMo3 for the complete joint.

Thanks & Regards

J.Gerald Jayakumar



On Friday, 23 December, 2022 at 04:35:28 pm IST, atul jha <atulkrjha21@gmail.com> wrote:


Dear sir
I Have to establish a PQR as per below detail :-

Material 1 : SA 516 gr 70 overlay of 3 mm by NiCrmo-3 ( done at vendor works).

Material 2 : A182 Gr F 44 UNS S 31254.
Code of construction ; B31.3.
Pwht : none 
I have to weld this joint in our plant as per attach figure.
QUERY: can a PQR with P1 to P8 by nicrmo-3 will serve the purpose OR I have to establish a PQR P1 ( cladded by nicrmo-3 ) to P8 welded by NicrMO-3 . I want to go with 1 st case
Does change in welding process also affect the above choice .
Kindly note that these vessel are for ARAMCO.
Kindly explain and guide me accordingly.
Regards
Atul jha 
B.E in welding Technology.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAC1tTUKXF5UizBMZH-tJTz7TDJtRaijzggwtJ4gCfbQxHGYP7Q%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1349670941.1982474.1671801255541%40mail.yahoo.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...