Use Double operator GTAW  ie two welders welding from either side simultaneously in 3G, pulling same weld puddle with Square butt joint,  5 mm gap.
Welders to practice first in 1 M long test plate. Use 2 or -2.4dia filler. 80/120 amps. 
Provide stiffnars to act gap closing . 1stStriking arc welder to add filler in joint gap second welder to operate at lower current level and add filler as and when required moving arc behind 3-4 mm from first welder. His arc also provide argon  shielding to weld  

On Thu, Jan 21, 2021, 08:43 Shahil Saini <sainishahil98@gmail.com> wrote:
Hello everyone, 

How to overcome the distortion in pressure vessel of material SS 304L?, having thickness 8mm of two dish-end and shell having thickness of 6 mm, I am attaching photographs of vessel for your reference,



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALfBO_931zTtSjSuhEit%3Dc-5afiAF3nAzqXgUU%3DK53y2oG6A_Q%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALfxFVLwYEPVAtOqBzSq-gz15ui8Z3o0242f4B-K4NzPQRNW1w%40mail.gmail.com.

No comments:

[MW:35742] PQR- Chemical testing requirements

Good Day to all, Reference std: ASME SEX IX Material ASTM A106 Gr B Pipe Dia and thickness: 2" and 8.74 mm. Service Fluid: Normal fluid...