Re: [MW:31923] SS-316L Rusting

Your issue has signs pointing to iron contamination. Iron contamination on the surface of the stainless steel will oxidize and begin the degradation processes on the contamination itself then upon the surface lattice of the metal. Effective passivation requires proper cleaning of the stainless steel followed by the removal of all free iron contamination from the surface. Our natural environment makes it so that the iron rusts immediately upon contact with air and or water. Once this happens, only a passivation treatment will stop the contamination and reverse the exposure. What I believe you need to focus on is the iron oxide removal process by means of either Phosphoric Acid or Acetic Acid treatment. I referred you to ASTM A967 on my previous email but am now recommending ASTM A380. Cannot stress enough how much cleanliness is needed for such situations. Hope it all works out for you. 

On Fri, Jan 8, 2021 at 11:59 PM Adnan B.BELGACEM <adnanbb.psi@gmail.com> wrote:
Dear Jamie;

Yes, the passive treatment meets the requirement of the ASTM and vendor instruction for application steps, we need to know the main reason for these faults could be due to the below reason which under investigation:

1- Vendor product used is expired (Under verification with supplier)
2- Water used was contaminated (checked and found acceptable)
3- Environment condition such as sunlight (maybe is not the main reason)
4- Other
So for this case, we need to repeat the passive application or we should follow another applicable procedure to remove this rust and to avoid the recurrence. 

regards
Adnan

Le jeu. 7 janv. 2021 à 04:49, Jamie Reyes <jamiejrmachineco@gmail.com> a écrit :
Did this material/fabrication receive chemical treatments such as, but not limited to, pickle and passivate treatment? If so, do you know what test method was used to prove conformance to specification? Do you have the inspection report from the pickling and passivation, if performed? Depending where you are located, ASTM A967 is an industry standard specification for such treatments that shall be followed, or its equivalence.   

On Wed, Jan 6, 2021 at 7:24 PM Adnan B.BELGACEM <adnanbb.psi@gmail.com> wrote:
Dear Expert,
Please could you advise about the root causes and how we can repair and stop this rust that occurred after the degreasing of the SS 304L tank? 

Regards
ABB


Le jeu. 28 mai 2020 à 13:30, sachit yadav <sachit.baroda@gmail.com> a écrit :
Appears to be fluid marks due to contamination or possibly poor pickling done.

On Thu, 28 May 2020, 10:46 Vinod Kataria, <vinod.kataria@blissanand.com> wrote:

Dear Expert,

We have received an email from our customer with pictures showing "rust" on the stainless steel (SS-316L) chambers.  Can anyone please tell me what you see in these pictures from your perspective?

 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/TY2PR0101MB29421148FFC32992DCB565C5878E0%40TY2PR0101MB2942.apcprd01.prod.exchangelabs.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAAT7JJiAe6oS4_WGLSW9_iN5bF6K2jOgVf6agTWSGipZ_e2DNw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAB68E5kHmYUDcySpQUz_PenstNbX6BH8aBxUMJUWLc%2BwPiQmBA%40mail.gmail.com.
--
Regards,
Jamie Reyes
J.R. Machine Company, Inc.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAB68E5kTUgZkfn%3DXVrcvnhSOne0%2B62-%2BGKdb2mwMR4-pEjJBvw%40mail.gmail.com.
--
Regards,
Jamie Reyes
J.R. Machine Company, Inc.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJNUtUNKgf_05GJmRHNymH9mM%2BHCH9tbyw8DS%2Bq_6ivzU2ipUg%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...