Dear Mr. Manish,

As in this case , you have the impact test requirement, then two separate PQRs shall be required for..

P.No 1, Gr.No 1 to P.No 1, G.No 1
P.No 1, Gr.No 2 to P.no 1, G.No 2

QW-403.5 states..
 
If materials differ only by group number (SAME P-number) and all other essential and supplementary essential variables are the same for two PQR's joining one group number to itself and the second group number to itself, then the dissimilar group number combination is considered to be qualified. So you can use these PQRs to qualify WPS for P.No 1 Gr.No 1 to P.No 1 to G.No 2.

Hope it clarifies 

Regards,
Atul Khatri
Principal Engineer- Piping
Haldor Topsoe India Pvt. Ltd


On Wed, Oct 21, 2020 at 8:42 PM Manish Kumar <mkmkr431@gmail.com> wrote:
Dear Sir,
With ref.. to the trailing email,P number is essential & Group number is supplementary variable,When impact value is required group number becomes essential. As per attachment of WPS & PQR  impact value is required at Heat affected zone.In this case,how will attached  PQR (P  number 1 & group number 2) be valid for P number 01 Group number 1 & 2.Pl advise me on this concern.


On Wed, Oct 21, 2020 at 8:06 PM Hany Nabil <eng.hanynabil20@gmail.com> wrote:
Dear Sir,

For your question 

Yes, a WPS is valid based on mentioned PQR as per ASME- IX code.

Because only P number essential variable and group number is not essential variable.


Thanks & Regards
Hany Nabil 

On Wed, Oct 21, 2020 at 4:12 PM Manish Kumar <mkmkr431@gmail.com> wrote:
Dear Sir,
If P number of material 1 & group number 1 & 2 is mentioned in WPS.While supporting relevant PQR is P number 1 & group number only 2. In this case,Will WPS be valid for relevant PQR.

Please advise us .

Attachment-
WPS & PQR 


--
Regards

Manish Kumar
Inspection(Mechanical) Engineer
PDIL-HURL Barauni site

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHfQ4k78r-LmTKgXVDyMf_9wE9PtMAo_C8QBbsd6aqpTaHWgwg%40mail.gmail.com.
--


 Best Regards,

 Eng. Hany Nabil
 Senior Welding Engineer
 Petrofac
 Engineering and Production Service
 Egypt Mobile: 002-01225622022




This message, including any attachments, may contain confidential and privileged information for the sole use of the intended recipient(s). Review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient, or authorised to receive information on behalf of the recipient, please contact the sender by reply email, and delete all copies of this message. While we have taken reasonable precautions to ensure that this message and any attachments are free from viruses, we cannot guarantee that they are virus free and accept no liability for any damage caused by this message or any attachments. Messages sent or received through our networks may be monitored to ensure compliance with the law, regulation and/or our policies.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAP1YJmRVwRqiLBh-PqJcbpDiq6GLMaDtgaAf%2BdrM_xhN6mrbxw%40mail.gmail.com.


--
Regards

Manish Kumar
Inspection(Mechanical) Engineer
PDIL-HURL Barauni site

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHfQ4k6TVRvBjzssM9D%2BrE%2BibHWvWakAfehAfR-mbNEHivjOkw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACKOSeCEBDYVPuptQYWhMDnEDhYPXEm39cuX-p9RhnQ5BzaydA%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...