Saturday, October 17, 2020

Re: [MW:31568] Welding of 410 Stainless Steel

Dear Vikas ji 
 tempering temp of 610°C ( 20°C below tempering temperature of the material).  

This PWHT temp is too low for softening martensite.
,make it at 720-730 Deg C for @2 hrs 

Regards


On Wed, Oct 14, 2020 at 7:15 PM Vikas Bhandari <vikas.bhandari349@gmail.com> wrote:
Hi

I am looking to weld 410 wrought stainless steel, there is a requirement to build up parent material because of incorrect machining.

AWS A 5.9 ER410 is the filler wire.

Considering the carbon and Chromium content, looking for a preheat of 200°C with maximum interpass as 315°C.

I take it ,No interruption during welding will be good for joint. Material will be constantly maintained at the minimum preheat temperature during welding.

 

For post weld heat treatment , I am thinking of bringing the material to 100°C (This is to ensure that there is complete transformation of the weld and HAZ to martensite ) and then follow this with PWHT for 4 hours.

 

I am thinking of tempering temp of 610°C ( 20°C below tempering temperature of the material).

 

Any recommendation in this regard will be greatly appreciated.


Thanks & best regards


Vikas

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACpSjO%3Dnw0gymJLohpEzJ3aWuz7y462ASyMioCY3KnMWXHb7Fw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3P1MgY5DsG5VVmaB2pSM5SYErfQY-UVMXHsL76tH%3DwQ7A%40mail.gmail.com.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...