1 - u can use 9018-D1 will give (20J @ -50C) CVN .. also after PWHT hardness will be around 200HV10 
2 - u can use 8018-C1 will give (20J @ -60C) CVN ... but Ni is not recommended in wet sour service 
so , you can go to 1st choice Mn-Mo elecreod

Best Regards ,
Ahmed Osman


On Monday, January 20, 2020, 09:33:10 a.m. GMT+3, Revdiwala Darshan <darshanmrevdiwala@gmail.com> wrote:


Dear Mr. Prakash,

Thanks for your reply, the details are mentioned below for your reference.

Impact required at MDMT -45
Service is Wet sour
There are different thicknesses from 20mm to 70mm.
PWHT Expected at 635 +/- 10 Deg.
PWHT Soaking Time max. 10 hours and Min. 1 hour.

Thanks & Regards,
Darshan

On Sun, 19 Jan 2020, 7:37 am 'Prakash Hegde' via Materials & Welding, <materials-welding@googlegroups.com> wrote:
Hi!
However what are the requirement?
Like
Impact test temp.Thk of weld n plate.Process being used . PWHT tem n time  consumables used
On this basis you can decide parameters and  precautions to be followed
Regards
Hegde



On Sun, 19 Jan 2020 at 7:29, Revdiwala Darshan
Dear Experts,

Can anyone suggest welding consumables for welding of SA 537 CL 2 ?

And precautions during welding.

Thanks,

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CABDq6ghMxsVcLvE9XAqhUQutToi5dP8_-x30A6RdUcjKdpzSfg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1239338402.2908207.1579405972304%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CABDq6gi8_r5C%2BDprVGZztSeScs_VN_N8fuZB66sZgoqXx3HLcw%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...