RE: [BULK]Re: [MW:30067] Aluminium welding failure from parent metal

I agree with Ramin's comment below.  Also from the attached test results you provided, the failure is in base metal. 

 

I suggest you to do a tensile test just with the base metal.  If the base metal comes lower in strength, it is not going to get improved by welding.

 

 

Feng Lu, Ph.D., NDE Level III
Metallurgy and Welding Engineer

Zachry Industrial, Inc.
3600 West Sam Houston Pkwy South

Suite 200

Houston, TX 77042

luf@zachrygroup.com
Office: 713.979.2648
Cell: 512 797 5777
www.ZachryGroup.com

This e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message.

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ramin Kondori
Sent: Sunday, September 15, 2019 8:27 PM
To: materials-welding@googlegroups.com
Subject: [BULK]Re: [MW:30063] Aluminium welding failure from parent metal

 

Normally, the specifications specify lower tensile strength levels for weld qualification test for these Aluminum grades (comparing to the original tensile strength of the parent metal); it is due to the softening effect of welding on Aluminum. 5754 plates are Al-Mg3 grades with subsequent work hardening and some tempering (quarter hard) and their welds (or HAZ) is weaker than the unaffected plate; it is normal. 

 

Having said that, I believe that with these results, you might be in the acceptable range. I recommend you to check your specification and confirm this point before proceeding. 

 

Ramin  Kondori

Sr. QA/QC & Welding Engineer

-----------------------------------------------------------

PG-Dip. in Welding Engineering (IWE  AT  0070)

BSc. in Civil Engineering (IUT)

BGAS Painting Inspector

ASNT Level I&II

                        

IIW-Logo-Colour-small

 

 

On Sun, Sep 15, 2019 at 5:31 PM <kadirgodil@gmail.com> wrote:

Dear experts,
EN AW 5754 H22 welded with ER5356, RT clear but gets failed in tensile.
What can be the reason please guide..
The artilce wleded is a 3 mm thick plate to plate butt joint.
Required YS 0.2 - 130 MPa
I am getting only 103 and 99 MPa.

Required UTS - 220-270 MPa
I am getting - 213 & 205 Mpa

Regards
Kadir godil

--
https://secure-web.cisco.com/15d1t2K3SDjWljsVjixiYCJQfTDqusQcTH3ppv9HObrUG9uVmeN8Epx-WPwrI8ZtbB_bxtPoydlACl3PNCTyXAmQMZn1tqSPCQbuOnT38sUwYKKteTDtFExAOoHjrFs4TJoFxsIyHOgdVTLGA977_7pJPkTqVKOk5-qiVishPOxmD58kV0kilCy1IUfS9i_-oc3_vUMOdS1qT3OZmeTCs6sr2YauOWudziGZB-r2FDzIPhlh-gNDaXmWgsDEJ4YE9FY2plj_UW-V5lhIbLrFC_GHFDzI9sLV3kR8SR6lEF6u_COPhBbWDM9NYehowhYE8UrcnQ5GtSAZh8oIvZFjgmpLDz7aF0yHHNQOtlOKeTyU/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1NlCQFjNRFtnQ-nsQ67ia4Qd29C-eVbNDc00LTPtkIqnPDbJZf88qk3x-_ooNnXzsibU65VeFHhhuMhHEYjexQn55alVxNwVvVh1d5kCPLlpKASpF7B-8S0PF_BCekOcSEusRdwFQcAD6tOX7vrzQ4vLJl-mIHb2neyx-oM57OVlGBsvUt9b3yGfCXNWKWj-hdwk0-vDdl25vFGrmjnfCX8zGA4gAjDudKnCMFviUYwI4Q9JR3tdtGTf-NPh4Kb9zvRM21KrJ3VXCw8fEDn7WT7aPurqO1WSEa6VD9aNsuGuNHa-ceitKmI9du4Jeu4YOkgJ4bdHDGi-ex7oWT1Kgeq1iLc6XX7lCaF2RW4p8PxQ/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://secure-web.cisco.com/1rRdEhAx-SDAKKdyQLZGUSQ0YwIhsmcWB5_6PX0_UdC19GqmPwVpiGCi9PiGP72uUPRkFcY0GFNI_sx9hq8bJTsRs-fhaFIc9mqQupgIpDNOP9-j9sCt_uqemuk4btPRYSQ1nwqBYP6Dv_AWDpPIG4AJM47NeT6syE3vDlb9Tcrm-QxJw_u6ojs5Hc_M6NE6wXxx3_q8D1NJ-ywMcVtwBH5Ac9dxRVeDxkknS_r2NdWy_5BtdI-nkFcpsB5VijY9_WRtwGa_RbymF5_fqSXdbUOC7rKMc56wNEIyHD82rAHBAeUAcF04uLp6_KTKXVoTh5QBRACjYkhMCa1KDE3KYHpFgln75HLDMkvWxuP1L3uM/https%3A%2F%2Fgroups.google.com%2Fd%2Fmsgid%2Fmaterials-welding%2F095b8b80-596a-4a0c-9cce-f2da1cbb7972%2540googlegroups.com.

--
https://secure-web.cisco.com/15d1t2K3SDjWljsVjixiYCJQfTDqusQcTH3ppv9HObrUG9uVmeN8Epx-WPwrI8ZtbB_bxtPoydlACl3PNCTyXAmQMZn1tqSPCQbuOnT38sUwYKKteTDtFExAOoHjrFs4TJoFxsIyHOgdVTLGA977_7pJPkTqVKOk5-qiVishPOxmD58kV0kilCy1IUfS9i_-oc3_vUMOdS1qT3OZmeTCs6sr2YauOWudziGZB-r2FDzIPhlh-gNDaXmWgsDEJ4YE9FY2plj_UW-V5lhIbLrFC_GHFDzI9sLV3kR8SR6lEF6u_COPhBbWDM9NYehowhYE8UrcnQ5GtSAZh8oIvZFjgmpLDz7aF0yHHNQOtlOKeTyU/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1NlCQFjNRFtnQ-nsQ67ia4Qd29C-eVbNDc00LTPtkIqnPDbJZf88qk3x-_ooNnXzsibU65VeFHhhuMhHEYjexQn55alVxNwVvVh1d5kCPLlpKASpF7B-8S0PF_BCekOcSEusRdwFQcAD6tOX7vrzQ4vLJl-mIHb2neyx-oM57OVlGBsvUt9b3yGfCXNWKWj-hdwk0-vDdl25vFGrmjnfCX8zGA4gAjDudKnCMFviUYwI4Q9JR3tdtGTf-NPh4Kb9zvRM21KrJ3VXCw8fEDn7WT7aPurqO1WSEa6VD9aNsuGuNHa-ceitKmI9du4Jeu4YOkgJ4bdHDGi-ex7oWT1Kgeq1iLc6XX7lCaF2RW4p8PxQ/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://secure-web.cisco.com/1z2zhm-r3jKgg6Od3muJ_PjGCu1R1mUizuvL7Go5RJ4e9MGiqIUeQi-JG0_AWfPV4xCsaX_kOe55oVyccYYTl5CZ0ig2bWiphnTeUePa8-b2JF7CFDn5JN_LGwXIUXq4o5VcoKclMcgdlgGZyUmQus_i50E1G6wjRzZiT8ICi77OPMogYQuV4UC6FMnWJeCHw47NBq7YkkxDsoEnSvkzYAbHFRgw5v7qpitjA5wgcnN9WAiqq0IYFx4Kxoj3WlzyLTTiETW4A74HZBecsnrb-2BL064giGUtsw6zMdPV9hkvqmfk5712b3iSPdQEL49vEmPSmLMtEkbgrhnP6vZc8WEQFVCs14z1QPs6Hj_rA_kQ/https%3A%2F%2Fgroups.google.com%2Fd%2Fmsgid%2Fmaterials-welding%2FCAEagfUi%253DnqBPCxoco_ev3N468FTr%252Bo41ugg-VeZs2_GnTraT3w%2540mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...