Sir why penning s not required in stellite? 

On Sun, 2 Jun 2019, 11:14 am Kannayeram Gnanapandithan, <kgpandithan@gmail.com> wrote:
For stellite peening is not required

On Sat, 1 Jun 2019 10:28 pm Gopalakrishnan G, <gopal2408@gmail.com> wrote:
Thickness is 90mm and penning for stress relieving ( heat stress)

On Thu, 30 May 2019, 6:45 pm Kannayeram Gnanapandithan, <kgpandithan@gmail.com> wrote:
Why are you doing penning? Not 100%. crack free possible if the hardness is more than 35HRC. Why preheat

On Wed, 29 May 2019 9:34 pm Gopalakrishnan G, <gopal2408@gmail.com> wrote:
Dear experts 
 Whether  it is possible to achieve crack free in stellite 6 welding?

I have a job in which I have to carry out hardfacing by stellite 6 and buffer layer with Tenalloy (E-7016).Preheating carried above 350c and interpass 250c with penning and after completion of welding job is covered by heating blanket.
 When I carry out dye penetrant crater cracks appears. But my client needs with 100% crack free.plz kindly give ur valuable guidelines. Thk u.


Regards
G.Gopalakrishnan 
 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOp_kKhugu9L6OHAss27tvndZhPOor%2BLHgGcBizCpiHe05O2uA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eN8cQKX53Zu3HpXnYtE6dbhJwqhuSwYaJUW%2BU56eXNnJw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOp_kKgGUupqJwhNL8K%2BCGEggg_o_GWA09258H8%3DZgd4Qjp-Gg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eNvq1%3Dimdk90Z7DUkku1MBX0W78%3DWCBJOPJztzLgv_o0Q%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOp_kKjUheqYij6-eku9Kn%3D_Z__ThE%3D8_OvSOc-bvhBVcMHcYQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...