all,
8" gate valve. wedge material
is carbon steel (A216 WCB). wedge harfaced
area became less thick due to wear.
1) can we remove original overlay and apply
13%chrome overlay ? in this case which
welding rod should we apply. if yes can you
please send me WPS for this ?
Ans:
yes u can removed.
you can qualified WPS on plate using 309L as buffer layer and 316L subsequent run
2) we can not able to trace the original
harfaced material b'se it is old valve. PMI is
showing Ni- 51% , Fe-25% and Cr- 18 %.
what is this material ?
Ans: may b due to long time in service its chemistry changed.
hope this help!!
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
Subscribe to:
Post Comments (Atom)
Re: [MW:35686] HDPE WPS
Refer ASME SEC IX There is separate chapter for Plastic welding . Based on that you have to prepare Sent from my iPhone On 21 Jun 2025, at...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment