Hi.

Duplex stainless steels have a good resistance to atmospheric corrosion as well as chloride corrosiin cracking.

But these steels are prone to form intermetallic compounds like sigma, chi.. These componds drastically reduce pitting resistance of duplex steels.

Sigma phase is a iron chromium compond (50-50). It reduces chromium levels in grain boundary areas and make steel susceptible to pitting.


It seems in your case also this is true. During welding of duplex steel you have encountered the temperature range in which these phases form.





On Friday, February 28, 2014, José Luís Ferreira <jluis.nf@gmail.com> wrote:
> Dear experts, 
> In my project, we're in trouble corrosion (pitting) in pipes SDSS (UNS S32750 / UNS 32760), the base metal is SDSS (UNS S32750 / UNS 32760), the fluid is seawater. Attached photos showing the defects. I would like someone to help me with technical information about the mechanisms that cause such defect, how to avoid and correct. 
> Regards,
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>  
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...