Sunday, February 23, 2014

Re: [MW:20165] Tube Expansion formula

Tube Thinning calculation
                                        Actual % Tube wall Thinning  = [(WTb-WTa)/WTb]  X 100                                          
WTb-Tube Wall Thickness before expanding = (Do-db)/2, Wta=Tube Wall Thickness after expanding=(Dh-da)/2
da=Tube ID after Expansion,db=Tube ID before Expansion,Dh=Diameter of tube Hole,Do=  OD of Tube.
Sl No Tube OD (DO) mm Tube ID (db) mm Tube ID after Expansion(da) mm Hole Size (Dh) mm % WallThinning  Remarks
1 42.54 33.07 33.84 42.71 6.34  
2 42.55 33.08 33.90 42.70 7.07  


On Sat, Feb 22, 2014 at 3:31 PM, Rahul Chaudhari <navyrahul@gmail.com> wrote:
Hi, 

Can somebody tell how to calculate tube expande,,,,,,
--
Thanks &  Warm Regards,

Rahul Chaudhari
 

P Think of the environment.

Please don't print this E- mail unless you really need to - this will help preserve trees on the earth.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...