Re: [MW:20103] Effect of higher Copper content on Austenitic Stainless Steels base material

Dear Prem:

I have personally observed hot shortness caused by Copper in cast ASS.
Material was an old Russian ASS and we were going to do some overlay welding. By the time the material temperature raised, one large crack opened immediately after welding. We conducted PMI and high Cu amount was evident.

Regards
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.kondori@petroyada.com
+98-2123592322
+98-9132150320



On Fri, Feb 14, 2014 at 7:36 PM, prem nautiyal <prem_nautiyal26@yahoo.com> wrote:
Hi Charley
 
Our job is a pressure vessel, MOC = 304L and the service is not for sulphuric acid, neither for elevated temp.
Its for a Nuclear Power Plant in India.
 
Our project specs. have restricted Copper content to 0.45% for ASS base materials. I was wondering what the reason could be for this.
 
Hence being from client side, I have kept the flanges and plates  of fabricator having Cu content greater than 0.45% on hold.
 
Regards
 
Prem Nautiyal
9769316004


On Friday, February 14, 2014 9:44 AM, Charley Sui <charleysui@gmail.com> wrote:
Prem,

Cu hasn't been traditionally added as alloying elements in austenitic stainless steel, this might be the reason why ASTM specs doesn't address Cu as a controlled element. due to an increased use of recycled SS and other Cu bearing alloys, elevated Cu content is observed but typically less than 1%.

Ahmad is right, Cu will increases the corrosion resistance against sulfuric acid (deliberately added in alloy 20 for such application), but Cu>0.8% may lead to hot shortness, some fabricators limit Cu below 0.5%.



On Mon, Feb 10, 2014 at 8:28 AM, prem nautiyal <prem_nautiyal26@yahoo.com> wrote:
Hi all
 
Vessel fabricator has offered SS flanges- SA 182F 304L and SA 240TP 304L plates.
 
After reviewing Lab check test reports and MTC  it is observed that Copper content is 0.60% for flanges and 0.69 % for plates. Copper content limits are not specified in the standard and I feel that the copper content is Not Traces and on higher side.
 
I have seen the max limit for copper specified for welding consumables in ASME Sec II-C, SFA 5.4 / 5.9. as 0.75%, but for base materials it is not specified in ASME Sec II-A or ASTM - A182.
 
 
I have kept the flanges and plate on hold.
 
I would like to know the effect of higher copper content on the SS base material and the reason for addition in SS plates and forgings.
 
Regards
 
Prem Nautiyal
9769316004
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to mailto:materials-welding%2Bunsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to mailto:materials-welding%2Bunsubscribe@googlegroups.com.

For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...