Friday, February 22, 2013

Re: [MW:16840] SS-304L Cladding on Inner Dia. of Carbon Steel ring

Cooling is not by water but by Air /Co2 gas surrounded by Jacket (Custom base)
Regards
Hegde

--- On Fri, 22/2/13, vineet kumar <vineet.rdb@gmail.com> wrote:

From: vineet kumar <vineet.rdb@gmail.com>
Subject: Re: [MW:16779] SS-304L Cladding on Inner Dia. of Carbon Steel ring
To: materials-welding@googlegroups.com
Cc: pb.hegde@yahoo.com
Date: Friday, 22 February, 2013, 10:27 AM

Dear,

Plz confirm,the Heat treatment of Cladded ring is necessary , my production engineer has recommended that we can use a local arrangement to cool the Ring at the time of cladding.

Cooling arrangement shall be - Water cooled by dipping the ring in the water tub.Heat is absorbed  by cooling water.

Plz recommend is it possible.

Regards,
Vineet 


On Saturday, February 16, 2013 9:52:31 PM UTC+5:30, Prakash Hegde wrote:
Hi!
My comments are given below
Regards

Prakash Hegde
08805593046

--- On Sat, 16/2/13, vineet kumar <vinee...@gmail.com> wrote:

From: vineet kumar <vinee...@gmail.com>
Subject: [MW:16779] SS-304L Cladding on Inner Dia. of Carbon Steel ring
To: material...@ googlegroups.com
Date: Saturday, 16 February, 2013, 10:50 AM

Dear Experts,

 

I have to made SS-304L Cladding on Inner Dia. of Carbon Steel ring , below are the details:

 

Base Metal - SA 516 Gr.70 

ID-490 mm , Thk-150 mm

 

Stainless Steel (304L)Cladding , thk- 5 mm finish 

 

Plz furnish my queries-

1) Method / process of Cladding. You can use GTAW or FCAW as per your availabilty of Automatic ID overlay facilty

2) Filler Wire/Electrode--E309LT1 for barrier +E308LT1 for subsequent layer if FCAW   and ER309L +ER308L for GTAW process

3) Heat treatment--For CS Pipe PWHT at Soaking tmp of 600-620C for 1hr soaking time which willbe suitable  up to 20Hrs soaking time

Howevr you require to qualify PQR to decide the height at

undilted chemistry of 308L is achieved from base of overlay

Regards,

Vineet Kumar

9971055188

--
To post to this group, send email to material...@ googlegroups.com
To unsubscribe from this group, send email to materials-weld...@ googlegroups.com
For more options, visit this group's bolg at http://materials-welding. blogspot.com/
http://www.linkedin.com/ groups/MaterialsWelding- 122787?home=&gid=122787&trk= anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@ googlegroups.com.
For more options, visit https://groups.google.com/ groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.