Friday, November 30, 2012

Re: [MW:16084] Consumable for SA 387 GR-12.CL2 materials

Hi!
NOT GOOD RESULT MEANS WHAT???????
Please let us know the exact problem you facer
For SA387 Gr12 C2 best suitable consumable is E8018B2 type Use g
ood brand Bholer,Kobelco,) (eg if you have problem with its mechanical properties which are strignent like Impact at minus 29C with higher value Some time better to use E8015 or 8016 type more of basic flux 
Hegde P.B.

--- On Thu, 29/11/12, sudalai kannan <sudalaims@gmail.com> wrote:

From: sudalai kannan <sudalaims@gmail.com>
Subject: [MW:16075] Consumable for SA 387 GR-12.CL2 materials
To: materials-welding@googlegroups.com
Date: Thursday, 29 November, 2012, 7:31 PM

Dear all,


I have a repair work on SA 387 GR-12.CL2 (75mm thick) materials, I tried with E8018-B2,but I didn't get good result. so can u give me suggestion which consumable is give good fusion and penetration for the above materials.


Thanks to all,


Regards,

M.Sudalai

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...