WPS qualified on groove welds can be used for weld build up as permitted by QW-202.3 of ASME SEC IX.

 

Existing WPS for groove welds can be revised to include weld metal build up.

 

Pls. check for insert plate option instead of weld build up in consultation with Design Engineer & Client.

 

Regards

Sudhir Kumar



On Wed, Nov 28, 2012 at 5:15 PM, welding <samirmehta.jnd@gmail.com> wrote:
Dear All,

Pls advice for following,

ASME b31.3 PIPING

1. by mistake my fabricator has made 4" hole in mother pipe (for branch connection) instead of 3", to overcome this issue he had weld (butter) the area by tig welding to meet actual requirement, somehow client came to know the issue and reject the spool, due to non availability of buttering procedure. we already have PQR for groove welding by tig process for same material.

pl advice what i can do in this regards, or to qualify procedure PIPE SIZE 54" THK 19 MM, also provide ref. std copy of procedure 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...