Monday, May 28, 2012

Re: [MW:14368] Hastalloy C pump casing repair

Hi,

It is indeed a casting defect, please specify the diameter of Pin Hole to evaluate its acceptance, As per ASME B16.34 Appendix 3, diamter more than 13mm is unacceptable.

Assuming weld repair is required, does client spec mandate solution annealing after weld repair? if not, don't go for it.

Secondly, you must refer the ASTM spec and name of Alloy correctly, which out of 4 mentioned below is the the alloy you are dealing with:

Hastelloy C-4 Alloy,C-22 Alloy,C-2000 Alloy,C-276 Alloy

Matching filler using GTAW process with proper joint preparation and stringer bead of low heat input, will do the job, below are matching filler metals for each of the alloy outlisted:

C-4 Alloy - ERNiCrMo-7
C-22 Alloy - ERNiCrMo-10
C-276 Alloy - ERNiCrMo-4
C-2000 Alloy - ERNiCrMo-17

Simply out of curiosity, what is the application, looks like Sulphuric Acid?


Cheers,
Manpreet Singh



On Sun, 27 May 2012 21:26:00 +0530 wrote
>Dear friends,

We have a pump casing made from Hastalloy C, a pin hole found in the

casing during leak testing. (it could be casting defect). Thickness at

pin hole location is approximately 2.5"-3".



Does anybody has some sort of repair ideas/procedures or any other

reference material.



regards,



--

To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Follow Rediff Deal ho jaye! to get exciting offers in your city everyday.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...