Now, my question is if i use the insulation painting (instead of classic one with insulation material+Jacket) on concerned SS pipe/vessel, could this replace this provision of coating?


2012/5/21 Ahmed Husain <ahmraha@yahoo.com>
This coating requirement on SS material is applied for lines or equipment requiring insualtion. 
.
Please refer below para of API 571 for prevention/mitigation of chloride stress cracking. One of the recomendation is coating of materials. Since CSCC is mostly associated with SS and nickel alloys, following recommendation is applicable to these matyerials.
 
 
 
4.5.1.6
Prevention / Mitigation
a) Use resistant materials of construction.
b) When hydrotesting, use low chloride content water and dry out thoroughly and quickly.
c) Properly applied coatings under insulation.
d) Avoid designs that allow stagnant regions where chlorides can concentrate or deposit.
e) A high temperature stress relief of 300 Series SS after fabrication may reduce residual stresses.
However, consideration should be given to the possible effects of sensitization that may occur,
increasing susceptibility to polythionic SCC, possible distortion problems and potential reheat cracking.
 
Regards,
 
Ahmed Husain
From: Lassaad Mokrani <lassaad.mokrani@gmail.com>
To: materials-welding@googlegroups.com
Cc: ahmraha@yahoo.com
Sent: Saturday, May 19, 2012 1:42 PM
Subject: Re: [MW:14313] COATING ON SS

Many thanks Mr.Ahmed,
Is the application of coating for either insulation and corrosion protection ok?


2012/5/19 Ahmed Husain <ahmraha@yahoo.com>
Dear Mr. Mokrani,
 
Many client specification and API standards or RP recommends application of coating on Stainless steel materials prior to insualtion to minimize/eliminate possibility of chloride stress corrosion cracking. This requirment is also in Aramco specification. 
 
Ahmed Husain

From: Lassaad Mokrani <lassaad.mokrani@gmail.com>
To: pgoswami <pgoswami@quickclic.net>; materials-welding@googlegroups.com
Sent: Friday, May 18, 2012 12:34 PM
Subject: [MW:14299] COATING ON SS

Gentelmen,
We are fabricating a SS 316L Fuel Gas scrubber 
For PP reasons, an insulation layer has to be applied. The client was asking to apply  an anticorrosion coating to the stainless steel material of the vessel for corrosion protection in marine environment.

In our experience we never did that for SS.

What do you think?. 
Is there any STD/Code that force that?

Design code: AMSE VIII Div 1
Location: Offshore Plateform


Meilleures salutations

Mokrani Lassaad
EPPM Sa.
00216 20 649 755
http://www.linkedin.com/pub/lassaad-mokrani/16/364/907


















P     Pensez environnement! N'imprimez ce mail que si c'est vraiment nécessaire
Please consider your environmental responsibility before printing this e-mail


This e-mail is confidential and it is intended only for the addressees. Any
review, dissemination, distribution, or copying of this message by persons
or entities other than the intended recipient is prohibited. If you have
received this e-mail in error, kindly notify us immediately by telephone or
e-mail and delete the message from your system. The sender does not accept
liability for any errors or omissions in the contents of this message which
may arise as a result of the e-mail transmission
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Meilleures salutations

Mokrani Lassaad
00216 20 649 755
http://www.linkedin.com/pub/lassaad-mokrani/16/364/907


















P     Pensez environnement! N'imprimez ce mail que si c'est vraiment nécessaire
Please consider your environmental responsibility before printing this e-mail


This e-mail is confidential and it is intended only for the addressees. Any
review, dissemination, distribution, or copying of this message by persons
or entities other than the intended recipient is prohibited. If you have
received this e-mail in error, kindly notify us immediately by telephone or
e-mail and delete the message from your system. The sender does not accept
liability for any errors or omissions in the contents of this message which
may arise as a result of the e-mail transmission
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Meilleures salutations

MOKRANI Lassaad
Consultant Civil Engineer
Tunisia
00216 20 649 755
http://www.linkedin.com/pub/lassaad-mokrani/16/364/907


















P     Pensez environnement! N'imprimez ce mail que si c'est vraiment nécessaire
Please consider your environmental responsibility before printing this e-mail


This e-mail is confidential and it is intended only for the addressees. Any
review, dissemination, distribution, or copying of this message by persons
or entities other than the intended recipient is prohibited. If you have
received this e-mail in error, kindly notify us immediately by telephone or
e-mail and delete the message from your system. The sender does not accept
liability for any errors or omissions in the contents of this message which
may arise as a result of the e-mail transmission

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...