Hi,

The pin hole leak could be  due to many factors.Since the product is a casting there could be other interlinked porosities. You may please take radiographs in the surrounding area to ensure that no other defects being present before proceeding further.

 Please see the link h2095 on repair recommendations of cast hastelloy.

What's the ASTM or hastelloy -C grade, C-4, C22, C276??

Appreciate your response.


Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist
Ontario, Canada.
Email-pgoswami@sympatico.ca,
pgoswami@quickclic.net


-----Original Message-----
From: materials-welding@googlegroups.com [
mailto:materials-welding@googlegroups.com] On Behalf Of ags 36681
Sent: Sunday, May 27, 2012 12:43 AM
To: materials-welding
Subject: [MW:14360] Hastalloy C pump casing repair

Dear friends,
We have a pump casing made from Hastalloy C, a pin hole found in the casing during leak testing. (it could be casting defect). Thickness at pin hole location is approximately 2.5"-3".

Does anybody has some sort of repair ideas/procedures or any other reference material.

regards,

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...