Hi Ghrab,
 
Corten is primarily a Copper added steel for weathering (atmospheric corrosion)  resistance, It comes in few grades,namely Coten -A & Corten-B. The default welding electrode which matches the BM chemistry is E-8018-W.
 
8018-C1 is (2.5%Ni) electrode, overallyed for Corten grades, not matching the BM chemistry. If the environment contains a lot of pollutants, there may be atmospheric corrosion overperiod of time.
 
Please find the data sheets for your help.
 
Thanks.
 
Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist & Consultant
Ontario,Canada.
Email-pgoswami@sympatico.ca,
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Zakaria ghrab
Sent: Thursday, October 20, 2011 5:17 AM
To: materials-welding@googlegroups.com
Subject: [MW:12727] May E8018-C1 substitue E8018-G to weld Corten Steel


Hi all

For welding Corten steel, we have in storage E8018-C1 Electrod, may it substitue  E8018-G, how can confirm ?

Regards
--
زكرياء غراب
GHRAB Zakaria
مسؤول عن الجودة
QA/QC SENAD
مشروع المحطة الحرارية ـ الوحدة الرابعة
المحمدية ـ المغرب

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...