Dear Rahuman,

 

In general, back purging is required for materials having Chromium > 3% in order to avoid oxide formation at the root. Please refer to AWS D10.8 for recommendations for welding of C-Mo steel piping and tubing.

 

Recommended filler metal is E8018-B8 (SFA 5.5)/ ER80S-B8 (SFA 5.28). For electrodes E8018-B8 type, suggested to use with low hydrogen type with H4 or H5 in order to control hydrogen level in weld metal.

 

The following precautions shall be adhered during welding qualification and further production welding.

 

  • Preheat upto 200 Deg. C
  • Max. interpass temperature is 300 Deg. C
  • Post heat the weld joint with 250-300 Deg. C for ½ to 1 hour for dehydrogenation purpose
  • PWHT around 750 – 760 Deg. C and holding time based on maximum thickness involved in production welds

 

Regards,

 

L. Prabhu kumar,

Sr. Principal Engineer,

 

Equipments & Materials Dept.,

Saipem India Projects Limited,

Nungambakkam High Road, Chennai - 600 034, India.

Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,

Mobile Ph. No.: +91 9003010978.


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of khadar.M. Rahuman
Sent: Wednesday, June 23, 2010 11:56 AM
To: materials-welding@googlegroups.com
Subject: [MW:5723] A335 Gr9

 

Gents.

 

 

Kindly advice A335 gr 9 material we do PQR...Client advice to Burging ...

 

1. If Burging need where is it mentioned..need to proof evidance.

2.  which electorde . what is the requirment  Pre heat and PWHT requirment..

 



 

Regards.

 

Muzib

QAQC - Incharge .

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

 




-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or 
entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged 
information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution 
or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If 
you have received this communication in error, please notify us immediately by responding to this email and then 
delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete 
transmission of the information contained in this communication nor for any delay in its receipt. 
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...