Wednesday, June 23, 2010

[MW:5722] RE: 5720] How to demagnetise the tube sheet?

Hi!

 Generally This grade does not get magnetized , unless  overlayed by ESSC , where high current being used. However you can demagnetized by

i)              This material  require preheating , through  thickness ( By electrical heating from circumference and front side )  to temperature of 150c

 

ii)             You can also demagnetize by winding cable around the tube sheet  with reversing the polarity  with high current of about 600Amp

 

 

Regards

 

Hegde P.B.

 

 

 

 

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Muhammed Ibrahim PK
Sent: Wednesday, June 23, 2010 3:19 PM
To: materials-welding@googlegroups.com
Subject: [MW:5720] How to demagnetise the tube sheet?

 

Hi Members,

 

We are suffering a problem in tube sheet. The tube sheet is P5A material (SA 336 Gr F22 CL.3) is magnetised.

 

We are not able to proceed the GTAW welding of tube to tube sheet.

 

We are not sure how it is happened. How can we demagnetise the tube sheet.

 

It is around 275 mm Thk and 3 mtr dia.

 

Kindly request the solution from experts.

Thanks & Regards
Muhammed Ibrahim PK

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...