Friday, February 26, 2010

RE: [MW:4387] ferrite number of duplex stainless steel weld

Anywhere between 40-60 for the weld and 35-55 for the HAZ should be acceptable... But the client normally has the last word on this issues.

-----Original Message-----
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Sukamal Naskar
Sent: 26 February 2010 05:22
To: materials-welding@googlegroups.com
Subject: Re: [MW:4376] ferrite number of duplex stainless steel weld

Optimum is 50FN, but 40 ~ 70 FN will be acceptable , but still it depends on the client's technical specifications.

Regards,

On 2/26/10, pankaj.johri@in.transport.bombardier.com
<pankaj.johri@in.transport.bombardier.com> wrote:
> Hi,
>
> We are welding duplex stainless steel.
>
> To control the parameters of welding, we are measuring ferrite number
> of weld.
>
> Can anybody tell us how acceptable values of ferrite numbers are decided.
>
>
> Regards,
>
> Pankaj
>
>
> Please consider the environment before you print / Merci de penser à
> l'environnement avant d'imprimer
>
> ______________________________________________________________________
> _________________________________________
>
> This e-mail communication (and any attachment/s) may contain
> confidential or privileged information and is intended only for the
> individual(s) or entity named above and to others who have been
> specifically authorized to receive it. If you are not the intended
> recipient, please do not read, copy, use or disclose the contents of
> this communication to others. Please notify the sender that you have
> received this e-mail in error by reply e-mail, and delete the e-mail
> subsequently. Please note that in order to protect the security of our
> information systems an AntiSPAM solution is in use and will browse through incoming emails.
> Thank you.
> ______________________________________________________________________
> ___________________________________________
>
>
> Ce message (ainsi que le(s) fichier(s)), transmis par courriel, peut
> contenir des renseignements confidentiels ou protégés et est destiné à
> l?usage exclusif du destinataire ci-dessus. Toute autre personne est,
> par les présentes, avisée qu?il est strictement interdit de le
> diffuser, le distribuer ou le reproduire. Si vous l?avez reçu par
> inadvertance, veuillez nous en aviser et détruire ce message. Veuillez
> prendre note qu'une solution antipollupostage (AntiSPAM) est utilisée
> afin d'assurer la sécurité de nos systèmes d'information et qu'elle
> furètera les courriels entrants.
> Merci.
> ______________________________________________________________________
> ___________________________________________
>
>
> --
> To post to this group, send email to
> materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding-unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views
> and meant for educational purposes only, Users must take their own
> decisions w.r.t. applicable code/standard/contract documents.
>


--
Sukamal

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


This e-mail and any attachment are confidential and may be privileged or otherwise protected from disclosure. It is solely intended for the person(s) named above. If you are not the intended recipient, any reading, use, disclosure, copying or distribution of all or parts of this e-mail or associated attachments is strictly prohibited. If you are not an intended recipient, please notify the sender immediately by replying to this message or by telephone and delete this email and any attachments permanently from your system.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...