Hello Mr Singh,

Single layer strip cladding solution is possible for SS347 with ES and SA process.
Depending on dimensions and requirements selection to be made :

SA-strip:
OERLIKON AST 300 - SUPRASTRIP 24 13LNb
OERLIKON AST 347 - SUPRASTRIP 24 13LNb

ES strip:
OERLIKON ELT 300 - SUPRASTRIP 21 11LNb (low speed)
OERLIKON ELT 300S - SUPRASTRIP 24 13LNb (high speed)
OERLIKON ELT 347-1 - SUPRASTRIP 19 9LNb (low speed)
 
In general the ES-strip cladding process can not garantue zero defects (PT-check) after machining in the ovelap zone. SA strip cladding process should be chosen in that case.
 
With kind regards,
Erwin GERING
AIR LIQUIDE WELDING


-----Oorspronkelijk bericht-----
Van: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Namens JASPAL SINGH
Verzonden: vrijdag 13 november 2009 6:03
Aan: Materials & Welding
Onderwerp: [MW:3644] Breesh-Lock Heat Exchangers Weld overlay


Dear all,

I have query regarding the Weld Overlay in Breesh Lock Heat
Exchanger.

As per specifications it is required to give SS347 Weld- overlay with
3mm undiluted chemistry . It is written that weld overlay shall be
lined & Faced. does it mean Strip cladding First then Machining.

Secondly is it possible to offer single layer solution for the same.

IS it required to machine the overlay in Breesh Lock Heat Exchanger.

Thanks in advance

Jaspal Singh


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...